Evaporation device and preparation method thereof
By designing through holes on the thermally conductive substrate and performing hydrophilic treatment, combined with a hydrophobic photothermal conversion layer, the directional precipitation of salt is achieved, solving the problem of efficiency reduction caused by salt deposition, improving evaporation efficiency and reducing energy consumption.
Patent Information
- Application Number
- CN202411138247.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-19
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-08-19
AI Technical Summary
In the existing seawater desalination technology, salt deposition on the photothermal conversion layer leads to a decrease in efficiency, and the equipment complexity and energy consumption are high, which limits its large-scale promotion and application.
Design multiple through-holes on the thermally conductive substrate, and perform hydrophilic treatment on the hole wall and bottom surface to cover the hydrophobic photothermal conversion layer to achieve directional precipitation of salt at the through-holes to avoid salting off covering the photothermal conversion layer.
It significantly improves evaporation efficiency, reduces energy consumption, and simplifies equipment design, avoids salt covering the photothermal conversion layer, ensuring efficient photothermal conversion performance.
Smart Images

Figure CN118908326A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of water treatment, and in particular relates to an evaporation device and a preparation method thereof. Background Art
[0002] Freshwater resources are precious natural resources that human society relies on for survival and development. With the continuous growth of the global population and the acceleration of industrialization, the demand for freshwater resources is increasing. However, surveys and studies have shown that about 97.5% of the water on the earth is seawater and cannot be directly drunk. The scarcity of freshwater resources makes the rational development and utilization of water resources a global challenge.
[0003] In order to alleviate the shortage of fresh water resources, people have developed a variety of seawater desalination technologies and sewage treatment technologies. These technologies mainly include reverse osmosis, multi-effect distillation, electrodialysis, etc., which can convert seawater or sewage into fresh water resources that can be used by humans. These technologies have alleviated the pressure on fresh water resources to a certain extent, but they have also brought a series of problems. First, these technologies require expensive infrastructure investment, which is a heavy economic burden for many countries and regions. Secondly, these technologies have huge energy demands, and a large amount of high-quality heat energy or high-quality electricity will be consumed during the implementation process, which not only increases operating costs, but also has a certain impact on the environment.
[0004] As a clean and renewable energy source, solar energy is gradually being used in the fields of seawater desalination and sewage treatment. Natural evaporation is one of the main sources of fresh water on land. Inspired by this, researchers began to explore the use of solar energy to drive water evaporation to improve the efficiency of fresh water acquisition. However, in reality, the poor light absorption performance of seawater, coupled with the barrier effect of salt, leads to low efficiency of natural evaporation, which limits the application and development of solar-driven water evaporation technology.
[0005] Therefore, it is necessary to provide a new solution to the above technical problems. Summary of the invention
[0006] The object of the present invention is to provide an evaporation device and a preparation method thereof, which have high evaporation efficiency and can reduce the influence of salt crystal precipitation on the photothermal interface during the evaporation process.
[0007] To achieve the above purpose, the technical solution provided by the present invention is as follows:
[0008] In a first aspect, the present invention provides an evaporation device, comprising: a thermally conductive substrate and a hydrophobic photothermal conversion layer; the thermally conductive substrate is provided with a plurality of through holes penetrating the top and bottom surfaces of the thermally conductive substrate, the bottom surface of the thermally conductive substrate and the hole walls of the through holes are hydrophilically treated; the hydrophobic photothermal conversion layer covers the top surface of the thermally conductive substrate.
[0009] In one or more embodiments, the hydrophobic photothermal conversion layer includes a hydrophobically modified photothermal conversion material, and the photothermal conversion material includes CoNiCuMnAl@C.
[0010] In one or more embodiments, the water contact angle of the hydrophobic light-to-heat conversion layer is greater than 90°; and / or the water contact angle of the bottom surface of the thermally conductive substrate and the hole wall of the through hole after hydrophilic treatment is less than 30°.
[0011] In one or more embodiments, the thickness of the thermally conductive substrate is 0.5-1 mm; and / or the diameter of the through hole is 2-5 mm.
[0012] In one or more embodiments, a water transfer layer is provided on the bottom surface of the thermally conductive substrate, and the water transfer layer is made of a water conductive material.
[0013] In one or more embodiments, a heat insulating layer is provided on the bottom surface of the water transfer layer, and the heat insulating layer is provided with a water transfer hole penetrating the top and bottom surfaces of the heat insulating layer, and the water transfer hole is filled with a water conductive filler, and the water conductive filler is in contact with the water transfer layer.
[0014] In a second aspect, the present invention provides a method for preparing an evaporation device, comprising:
[0015] A thermally conductive substrate and a photothermal conversion material are prepared, wherein a plurality of through holes penetrating the top and bottom surfaces of the thermally conductive substrate are provided; the photothermal conversion material is hydrophobically modified; the hydrophobically modified photothermal conversion material is deposited on the top surface of the thermally conductive substrate; and the bottom surface of the thermally conductive substrate and the hole walls of the through holes are hydrophilically treated.
[0016] In one or more embodiments, the preparation method of the thermally conductive substrate includes:
[0017] The top surface of the thermal conductive substrate is scanned and engraved using a laser to form a micron-level groove structure on the top surface of the thermal conductive substrate; after the scanning and engraving is completed, the thermal conductive substrate is cleaned and dried.
[0018] In one or more embodiments, the photothermal conversion material is prepared by:
[0019] Weigh cobalt acetate, nickel acetate tetrahydrate, copper acetate monohydrate, and manganese acetate, add them to N,N-dimethylformamide, stir evenly, and obtain a mixed solution A; add terephthalic acid to the mixed solution A, stir vigorously for 1 to 3 hours, and obtain a mixed solution B; centrifuge the mixed solution B to obtain a precipitate; use N,N-dimethylformamide to centrifuge and wash the precipitate, collect the precipitate and vacuum dry it; grind the dried precipitate into powder to obtain a high entropy alloy MOF precursor; transfer the high entropy alloy MOF precursor material to a tube furnace, and heat it in an argon hydrogen atmosphere. Under the condition of mixed gas, the furnace temperature is raised to 680-720°C at a heating rate of 5°C per minute, and after calcination for 1-2 hours, the temperature is lowered to room temperature to obtain a calcined black powder; the calcined black powder is added to a dilute sulfuric acid solution with a concentration of 3-6 mmol / L, and ultrasonically dispersed to obtain a mixed solution C; the mixed solution C is placed in an environment of 60-80°C, and impurities in the black powder are etched by sulfuric acid; after etching, the mixed solution C is centrifuged, a black precipitate is collected, washed, and dried to obtain a CoNiCuMnAl@C photothermal conversion material.
[0020] In one or more embodiments, the hydrophilic treatment method of the bottom surface of the thermally conductive substrate and the hole wall of the through hole includes: scanning the bottom surface of the thermally conductive substrate and the hole wall of the through hole by laser.
[0021] Compared with the prior art, the evaporation device and preparation method provided by the present invention can significantly improve the evaporation efficiency of the evaporation device by providing a plurality of through holes penetrating the top and bottom surfaces of the thermally conductive substrate, performing hydrophilic treatment on the bottom surface of the thermally conductive substrate and the hole walls of the through holes, so that the hydrophobic photothermal conversion layer covers the top surface of the thermally conductive substrate, and can realize the directional precipitation of salt crystals at the through holes, thereby avoiding salt precipitation on the photothermal conversion layer and affecting the photothermal conversion efficiency of the photothermal conversion layer. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the prior art descriptions are briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention, and for ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0023] Figure 1 It is a schematic diagram of the structure of an evaporation device in one embodiment of the present invention;
[0024] Figure 2 This is a morphology diagram of the hydrophobically modified photothermal conversion material prepared in Example 1 of the present invention;
[0025] Figure 3 This is a comparison chart of the evaporation amounts of the evaporation devices prepared in Examples 1 to 3 of the present invention;
[0026] Figure 4 This is a comparison chart of the evaporation amounts of the evaporation devices prepared in Example 2 of the present invention and Comparative Example 1;
[0027] Figure 5 This is a diagram of the salting-out state of the evaporation device prepared in Example 1 of the present invention after a 180-minute test;
[0028] Figure 6 This is a diagram of the salting-out state of the evaporation device prepared in Example 1 of the present invention every 10 minutes;
[0029] Figure 7 This is a diagram of the salting-out state of the evaporation device prepared in Example 2 of the present invention after a 180-minute test;
[0030] Figure 8 The salting out state diagram of the evaporation device prepared in Example 2 of the present invention every 10 minutes
[0031] Fig. 9 This is a diagram of the salting-out state of the evaporation device prepared in Example 3 of the present invention after a 180-minute test;
[0032] Fig.10 This is a diagram of the salting-out state of the evaporation device prepared in Example 3 of the present invention every 10 minutes.
[0033] Description of main reference numerals:
[0034] 11-heat-conducting substrate, 111-through hole, 12-hydrophobic light-to-heat conversion layer, 13-water transport layer, 14-heat-insulating layer, 15-water-conducting filler. DETAILED DESCRIPTION
[0035] In order to enable those skilled in the art to better understand the technical solutions in the present invention, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.
[0036] It should be noted that, unless otherwise indicated, all numbers used in the specification and claims to represent feature sizes, quantities and physical properties should be understood to be modified by the term "about" in all cases. Therefore, unless otherwise indicated, the numerical parameters listed in the above specification and the attached claims are approximate values, and those skilled in the art can use the teachings disclosed herein to seek to obtain the desired properties and appropriately change these approximate values. The use of numerical ranges expressed as endpoints includes all numbers within the range and any range within the range, for example, 1 to 5 includes 1, 1.2, 1.4, 1.55, 2, 2.75, 3, 3.80, 4 and 5, etc.
[0037] As the global freshwater shortage becomes increasingly serious, seawater desalination technology has become an important means for humans to obtain fresh water. However, although existing seawater desalination technologies, such as reverse osmosis, multi-effect distillation and electrodialysis, can alleviate the shortage of freshwater resources to a certain extent, they still have many problems in their application, such as high equipment cost, high energy consumption, and reduced efficiency due to salt deposition.
[0038] A prominent problem in the prior art is that salt is deposited on the photothermal conversion layer, resulting in a significant decrease in the photothermal conversion efficiency, which in turn affects the efficiency of the entire evaporation process. This is because the accumulation of salt will cover the photothermal conversion layer, hindering its ability to absorb solar energy. In addition, the complexity of the equipment in the prior art and the high operating and maintenance costs also limit its large-scale promotion and application. Therefore, how to reduce energy consumption and simplify equipment design while improving evaporation efficiency has become a technical problem that needs to be solved urgently.
[0039] The technical implementation idea of the present invention is to propose a new evaporation device through innovative structural design and material selection, aiming to effectively solve the problems in the above-mentioned prior art. The core idea of the present invention is to use the combination of hydrophilicity and hydrophobicity on both sides of the device to achieve directional growth of salt during the evaporation process, avoid salt covering the photothermal conversion layer, and thus improve the photothermal conversion efficiency and evaporation efficiency.
[0040] Specifically, the present invention designs multiple through holes that penetrate the top and bottom surfaces on the thermally conductive substrate, and performs hydrophilic treatment on the hole walls and bottom surfaces of the through holes, while covering the top surface of the thermally conductive substrate with a hydrophobic photothermal conversion layer. Under this structure, the liquid can quickly enter the through hole through the hydrophilic hole walls, while the salt will grow directionally on the hole walls during the evaporation process to avoid covering the photothermal conversion layer. This innovative design can not only improve the evaporation efficiency, but also reduce energy consumption and simplify the complexity of the equipment.
[0041] Please refer to Figure 1As shown, an evaporation device in an embodiment of the present invention comprises a heat-conducting substrate 11 and a hydrophobic light-to-heat conversion layer 12. The heat-conducting substrate 11 is provided with a plurality of through holes 111 penetrating the top and bottom surfaces of the heat-conducting substrate 11, and the bottom surface of the heat-conducting substrate 11 and the hole walls of the through holes 111 are hydrophilically treated; the hydrophobic light-to-heat conversion layer 12 covers the top surface of the heat-conducting substrate 11.
[0042] It should be noted that the heat-conducting substrate 11 of the evaporation device is provided with a plurality of through holes 111 penetrating the top surface and the bottom surface. The bottom surface of the heat-conducting substrate 11 and the hole walls of the through holes 111 are hydrophilic treated to have good wettability. When the evaporation device contacts the liquid, the liquid can quickly wet the hole walls and enter the through holes 111. This design allows the liquid to fully contact each through hole 111 of the substrate, thereby providing sufficient liquid supply for the subsequent evaporation process.
[0043] The top surface of the heat-conducting substrate 11 is covered with a hydrophobic photothermal conversion layer 12. The hydrophobic design can effectively prevent the liquid from forming a continuous liquid film on the photothermal conversion layer, thereby preventing salt from precipitating and covering the photothermal conversion layer. This design ensures that the photothermal conversion layer is always exposed to the air, can absorb solar energy to the maximum extent and convert it into heat energy, and improve evaporation efficiency.
[0044] One side of the evaporation device is hydrophilic (pore wall and bottom surface), and the other side is hydrophobic (top surface). This structure can effectively control the precipitation position of salt during the evaporation process. Since the hydrophilic pore wall can attract and retain liquid, the salt will gradually precipitate on the pore wall during the evaporation process and grow in a directional manner toward the top surface of the substrate.
[0045] When salt crystals begin to grow on the hole wall, a thin liquid film will exist on the surface of the salt crystals. This liquid film can continuously transport liquid to the surface of the salt crystals, allowing new salt crystals to continue to grow above the original salt crystals. This directional growth mechanism can effectively control the salt in the through hole 111 area, thereby avoiding the deposition of salt on the photothermal conversion layer, and ensuring that the photothermal conversion layer always maintains efficient photothermal conversion performance and is not affected by salt coverage.
[0046] Specifically, when the evaporation device contacts the liquid (such as seawater), the liquid first wets the bottom surface of the thermally conductive substrate 11 and the hole wall surface of the through hole 111. This is because the hole wall has been hydrophilic and has strong wettability, so that the liquid can quickly penetrate and fill the through hole 111. The hydrophilic surface can attract water molecules and ensure that the liquid is evenly distributed on the hole wall surface, thereby providing sufficient liquid supply for the evaporation process.
[0047] As the evaporation process continues, water molecules evaporate continuously on the surface of the pore wall and the surface of the liquid in the pore. Since the pore wall is hydrophilic, the liquid will evaporate preferentially along the pore wall, and this process will cause the salt to gradually concentrate and precipitate on the surface of the pore wall. The precipitation of salt occurs first on the pore wall because the liquid on the pore wall is easier to evaporate than the liquid in the through hole 111.
[0048] When salt begins to precipitate on the surface of the pore wall and forms initial salt crystals, a very thin liquid film will form on the surface of the salt crystals. The liquid film can continue to transport liquid to the surface of the salt crystals. This is because the liquid film has a capillary effect that can attract and retain water molecules, so that the liquid is continuously supplied to the surface of the salt crystals. As the water in the liquid film continues to evaporate, new salt will continue to precipitate and grow on the original salt crystals. This process forms the phenomenon of salt growing directional along the pore wall.
[0049] Since the salt mainly grows directionally on the surface of the pore wall and in the pores, and the hydrophobic photothermal conversion layer 12 on the top surface of the thermal conductive substrate 11 is not easily wetted by liquid, the salt will not precipitate on the photothermal conversion layer. This design effectively prevents the salt from covering the photothermal conversion layer, ensuring that the photothermal conversion layer is always exposed to the air, which can maximize the absorption of solar energy and convert it into heat energy, thereby improving the evaporation efficiency.
[0050] In an exemplary embodiment, the hydrophobic photothermal conversion layer 12 includes a hydrophobically modified photothermal conversion material, and the photothermal conversion material includes CoNiCuMnAl@C (carbon-wrapped high entropy alloy). High entropy alloys are alloys formed by mixing multiple elements in a nearly equiatomic ratio and have excellent thermal stability and mechanical properties. During the photothermal conversion process, high entropy alloys can withstand high temperatures without performance degradation. Carbon materials have excellent photothermal conversion efficiency and chemical stability. The carbon-wrapped structure not only improves the photothermal stability of the high entropy alloy, but also enhances its ability to absorb solar energy.
[0051] The core performance of photothermal conversion materials is their efficiency in converting light energy into heat energy. Carbon-wrapped high-entropy alloys (CoNiCuMnAl@C) have excellent photothermal conversion performance. Due to their complex composition and structure, high-entropy alloy materials can efficiently absorb solar energy over a wide band and quickly convert it into thermal energy. At the same time, carbon materials have high light absorption efficiency and thermal conductivity, which further improves the photothermal conversion efficiency. Moreover, high-entropy alloy materials have excellent thermal stability and corrosion resistance, and can maintain stable performance in high temperature and corrosive environments. This enables the photothermal conversion layer to be used for a long time without being affected by environmental factors.
[0052] In an exemplary embodiment, the water contact angle of the hydrophobic light-to-heat conversion layer 12 is greater than 90°; the water contact angles of the bottom surface of the thermally conductive substrate 11 and the hole wall of the through hole 111 after hydrophilic treatment are less than 30°.
[0053] The design goal of the hydrophobic photothermal conversion layer 12 is to prevent the liquid from forming a liquid film on the surface, thereby ensuring the photothermal conversion efficiency. The water contact angle is an important parameter for measuring the wettability of a surface. A contact angle greater than 90° indicates that the surface has a high hydrophobicity, that is, water droplets form a sphere on the surface without spreading. The hydrophobic surface can prevent the liquid from covering the photothermal conversion layer, ensuring that its surface is always exposed to the air. In this way, the photothermal conversion layer can absorb solar energy to the maximum extent and efficiently convert it into heat energy for water evaporation.
[0054] The hydrophobic surface prevents the liquid from spreading and staying on the photothermal conversion layer, thereby preventing salt from precipitating on the photothermal conversion layer. This design effectively prevents salt from covering the photothermal conversion layer, maintaining its long-term and efficient photothermal conversion ability. In addition, the hydrophobic surface has a self-cleaning property, and water droplets can carry away dust and impurities on the surface when rolling on the surface. This property helps to maintain the cleanliness of the photothermal conversion layer and further improve its photothermal conversion efficiency.
[0055] The bottom surface of the thermal conductive substrate 11 and the hole wall of the through hole 111 are treated with hydrophilicity, and the water contact angle is less than 30°, indicating that it has strong hydrophilicity, that is, the liquid can spread quickly on the surface. The hydrophilic thermal conductive substrate 11 can quickly attract the liquid and evenly distribute the liquid on the hole wall and the bottom surface. This design ensures that there is sufficient liquid supply during the evaporation process, thereby maintaining continuous water evaporation. During the evaporation process, the liquid first evaporates on the hydrophilic hole wall, and the salt gradually precipitates on the hole wall.
[0056] Due to the hydrophilicity of the pore wall, salt can grow in a directional manner on the pore wall and avoid covering the photothermal conversion layer. The design of the hydrophilic pore wall allows salt to gradually accumulate on the pore wall surface and grow outside the pore, thereby achieving effective control of salt precipitation. In addition, the hydrophilic surface can increase the diffusion rate of water molecules and accelerate the flow and evaporation process of the liquid on the pore wall. This design can significantly improve the evaporation efficiency, allowing the evaporation device to evaporate more water per unit time.
[0057] In an exemplary embodiment, the thickness of the thermally conductive substrate 11 is 0.5-1 mm; the diameter of the through hole 111 is 2-5 mm.
[0058] The main function of the heat-conducting substrate 11 is to effectively conduct the solar energy absorbed by the light-heat conversion layer to the liquid, causing it to evaporate quickly. A moderate thickness (0.5-1 mm) can ensure that the substrate has sufficient mechanical strength and heat conduction capacity. If the substrate is too thick, the heat conduction efficiency will be reduced, affecting the evaporation rate; if it is too thin, the mechanical strength of the substrate is insufficient and it is easy to be damaged during use.
[0059] The moderate aperture design of through hole 111 (2-5 mm) facilitates the directional precipitation of salt on the pore wall. The smaller pore size provides sufficient surface area, allowing the salt to gradually grow along the pore wall without forming a cover on the photothermal conversion layer. This design ensures the directional precipitation process of salt on the pore wall, thereby avoiding the problem of the photothermal conversion layer being covered by salt and maintaining efficient photothermal conversion performance.
[0060] If the pore size is too small (less than 2mm), it is easy to be blocked due to salt precipitation or impurity accumulation. Once the pore is blocked, the liquid supply is blocked and the evaporation efficiency will be significantly reduced. Therefore, choosing a pore size within the range of 2 to 5mm can effectively avoid the blockage problem and ensure that the liquid can pass through the pore wall smoothly during the evaporation process.
[0061] Apertures that are too large will reduce the effective photothermal conversion area and affect evaporation efficiency. A larger aperture means that fewer holes need to be opened on the substrate, which reduces the effective area of the photothermal conversion layer, reduces the absorption of solar energy and the conversion efficiency of thermal energy. Therefore, an aperture between 2 and 5 mm can maximize the number and distribution of holes while preventing clogging, thereby optimizing photothermal conversion and evaporation efficiency.
[0062] In an exemplary embodiment, a water transfer layer 13 is provided on the bottom surface of the thermally conductive substrate 11 , and the water transfer layer 13 is made of a water conductive material.
[0063] The core function of the evaporation device is to absorb solar energy through the photothermal conversion layer and convert it into heat energy for water evaporation. In order to maintain an efficient evaporation process, it is necessary to ensure that liquid (such as seawater) can be continuously and stably supplied to the bottom surface of the thermal conductive substrate 11 and the hole wall of the through hole 111.
[0064] The water transfer layer 13 is provided to ensure that the liquid can be continuously directed to the bottom surface of the heat-conducting substrate 11. The water transfer layer 13 is made of a water-conducting material (such as absorbent cotton), which usually has a high capillary force and can attract and conduct water. Through the water transfer layer 13, the liquid can be quickly and evenly distributed on the bottom surface of the heat-conducting substrate 11, thereby ensuring that the evaporation device is always in the best working state.
[0065] The water transfer layer 13 can evenly distribute the liquid to the bottom surface of the thermally conductive substrate 11 and the hole wall of the through hole 111 through its water conductivity. The water-conducting material usually has good wettability and capillary action, and can quickly absorb the liquid and conduct it along the direction of the water transfer layer 13. This design ensures that the liquid is evenly distributed on the entire bottom surface of the thermally conductive substrate 11, optimizing the evaporation process.
[0066] Specifically, a heat insulating layer 14 is provided on the bottom surface of the water transfer layer 13 . The heat insulating layer 14 is provided with a water transfer hole penetrating the top and bottom surfaces of the heat insulating layer 14 . The water transfer hole is filled with a water conductive filler 15 . The water conductive filler 15 is in contact with the water transfer layer 13 .
[0067] The evaporation process relies on the photothermal conversion layer to convert solar energy into thermal energy, thereby heating the liquid and promoting evaporation. The provision of the thermal insulation layer 14 can prevent the thermal conductive substrate 11 and the water transfer layer 13 from being in direct contact with the water body, prevent the heat energy from being carried away by the water body at the bottom, and reduce the overall evaporation efficiency. The thermal insulation layer 14 can effectively prevent the heat energy from being conducted downward and reduce the heat energy loss. By providing the thermal insulation layer 14 on the bottom surface of the water transfer layer 13, it can be ensured that the heat energy is concentrated near the thermal conductive substrate 11 and the photothermal conversion layer, thereby improving the evaporation efficiency.
[0068] The heat insulating layer 14 is provided with water transfer holes penetrating the top and bottom surfaces, and these water transfer holes are used to conduct water, so that liquid can be transported from the water body to the water transfer layer 13 through the heat insulating layer 14. The water conducting filler 15 (such as absorbent cotton) has good capillary action, can attract and retain liquid, and transport it from the water body to the water transfer layer 13. Through the capillary action, the water conducting filler 15 can continuously supply liquid to ensure an uninterrupted evaporation process.
[0069] The material of the heat insulation layer 14 is preferably polystyrene foam. Polystyrene foam has good thermal resistance and can effectively prevent heat conduction. At the same time, polystyrene foam has low density and good buoyancy, so that the evaporation device can float on the water.
[0070] In one embodiment of the present invention, a method for preparing the aforementioned evaporation device is provided, and the method specifically comprises the following steps:
[0071] S201: preparing a thermally conductive substrate and a photothermal conversion material, wherein the thermally conductive substrate is provided with a plurality of through holes penetrating the top surface and the bottom surface thereof.
[0072] The thermal conductive substrate is usually made of materials with high thermal conductivity, such as metals such as aluminum and copper, or ceramic materials with high thermal conductivity. These materials can conduct heat quickly, thereby improving evaporation efficiency. There are multiple through holes penetrating the top and bottom surfaces of the thermal conductive substrate, with a hole diameter ranging from 2 to 5 mm. The purpose of the through hole design is to provide a path for liquid evaporation and promote the directional precipitation of salt on the hole wall.
[0073] Photothermal conversion materials need to have efficient photothermal conversion capabilities, such as carbon-wrapped high-entropy alloys (CoNiCuMnAl@C). This material has excellent light absorption properties in a wide range of wavelengths and can quickly convert light energy into heat energy.
[0074] In an exemplary embodiment, the preparation method of the thermal substrate specifically includes: using a laser to scan the top surface of the thermal conductive substrate to form a micron-level groove structure on the top surface of the thermal conductive substrate; after the scanning is completed, the thermal conductive substrate is cleaned and dried.
[0075] The micron-scale groove structure can significantly increase the surface area of the thermally conductive substrate, thereby improving the adhesion of the photothermal conversion layer. This structure provides more attachment points for the photothermal conversion material, ensuring that its deposition is more uniform and stable. The groove structure is conducive to reducing the reflection and scattering of light, allowing more light energy to be absorbed and utilized, enhancing the light absorption capacity of the photothermal conversion layer, and improving the photothermal conversion efficiency.
[0076] During the laser scanning process, tiny particles, melts and other impurities may remain on the surface of the substrate, which will affect the deposition quality and adhesion performance of the photothermal conversion layer. A cleaning step can be performed to ensure the cleanliness of the substrate surface. Cleaning methods can include ultrasonic cleaning, chemical solvent cleaning and deionized water cleaning. Ultrasonic cleaning uses high-frequency vibration to remove surface attachments, chemical solvents can dissolve organic matter, and deionized water cleaning can remove inorganic particles and ionic impurities.
[0077] In an exemplary embodiment, the preparation method of the photothermal conversion material specifically includes: weighing cobalt acetate, nickel acetate tetrahydrate, copper acetate monohydrate, and manganese acetate, and adding them to N, N-dimethylformamide, stirring evenly to obtain a mixed solution A; adding terephthalic acid to the mixed solution A, and vigorously stirring for 1 to 3 hours to obtain a mixed solution B; centrifuging the mixed solution B to obtain a precipitate; centrifuging and washing the precipitate with N, N-dimethylformamide, collecting the precipitate and vacuum drying; grinding the dried precipitate into powder to obtain a high entropy alloy MOF (metal organic framework) precursor; The OF precursor material is transferred to a tube furnace, and under the condition of argon-hydrogen mixed gas, the furnace temperature is raised to 680-720°C at a heating rate of 5°C per minute, and after calcination for 1-2 hours, the temperature is cooled to room temperature to obtain a calcined black powder; the calcined black powder is added to a dilute sulfuric acid solution with a concentration of 3-6 mmol / L, and ultrasonically dispersed to obtain a mixed solution C; the mixed solution C is placed in an environment of 60-80°C, and impurities in the black powder are etched by sulfuric acid; after the etching is completed, the mixed solution C is centrifuged, and the black precipitate is collected, washed, and dried to obtain a CoNiCuMnAl@C photothermal conversion material.
[0078] S202: Performing hydrophobic modification on the photothermal conversion material.
[0079] By hydrophobic modification of the photothermal conversion material, a hydrophobic coating can be formed on the surface of the material, making the water contact angle greater than 90°. The purpose of hydrophobic treatment is to prevent the liquid from forming a liquid film on the surface of the photothermal conversion material, thereby ensuring that the surface of the material is always exposed to the air and maximizing the photothermal conversion efficiency. In addition, the hydrophobic surface can reduce the deposition of salt on the surface of the material and extend the service life of the device.
[0080] In an exemplary embodiment, the hydrophobic modification method includes: weighing the photothermal conversion material, injecting an ethanol solution containing 3 wt % hexadecyltrimethoxysilane, and ultrasonically dispersing it; centrifuging the solution using a centrifuge, and placing the precipitate in an oven to dry.
[0081] Hexadecyltrimethoxysilane (HDTMS) has a long-chain alkyl group (C16) and a trimethoxysilane group. The long-chain alkyl group provides hydrophobicity, while the trimethoxysilane group can form a chemical bond with the surface of the material, thus making the surface stable and hydrophobic. The trimethoxysilane group can form a strong silicon-oxygen bond (Si-O-Si) with the hydroxyl group (-OH) or other reactive groups on the surface of the material through hydrolysis and condensation reactions, ensuring the stability and durability of the hydrophobic layer.
[0082] S203: depositing the hydrophobically modified photothermal conversion material on the top surface of the thermally conductive substrate.
[0083] The hydrophobically modified photothermal conversion material can be configured into an electrophoretic deposition liquid, and the photothermal conversion material can be deposited on the top surface of the thermally conductive substrate by electrophoretic deposition to form a photothermal conversion layer.
[0084] Electrophoretic deposition is a method that uses an electric field to move charged particles in a solution and deposit them on an electrode. Under the action of the electric field, the deposited particles move along the direction of the electric field and form a uniform coating on the target substrate (electrode).
[0085] The thermally conductive substrate can be used as a working electrode (cathode or anode). The photothermal conversion material particles carry an electric charge (positive or negative) in the solution. Under the action of an external electric field, the charged particles move to the surface of the thermally conductive substrate and deposit on it to form a uniform coating.
[0086] S204: performing hydrophilic treatment on the bottom surface of the thermally conductive substrate and the hole walls of the through holes.
[0087] The purpose of hydrophilic treatment is to ensure that the liquid can quickly wet the bottom surface of the thermal conductive substrate and the through-hole wall, thereby forming a specific vapor path and achieving directional precipitation of salt during evaporation. The hydrophilic surface can attract liquid and promote its rise along the hole wall, thereby achieving uniform distribution and continuous supply of liquid, ensuring the continuity and efficiency of the evaporation process.
[0088] In an exemplary embodiment, the hydrophilic treatment method of the bottom surface of the thermally conductive substrate and the hole wall of the through hole includes: scanning the bottom surface of the thermally conductive substrate and the hole wall of the through hole by laser.
[0089] Laser scanning uses a high-energy laser beam to perform micro-processing on the surface of a material. The laser beam can form micro-nano structures on the surface of the material, increasing the surface area. At the same time, the high temperature causes the chemical bonds on the surface of the material to change, forming more hydrophilic groups (such as hydroxyl groups). Laser scanning can form micro-nano grooves and protrusions on the surface of the thermally conductive substrate. These microstructures increase the surface roughness and specific surface area. Rough surfaces are more likely to capture and retain water molecules, thereby increasing the hydrophilicity of the material. The presence of microstructures enhances the capillary action of the surface, and water molecules can more easily diffuse and wet between these structures, further improving the hydrophilic properties.
[0090] The present invention will be further described below in conjunction with specific embodiments.
[0091] Example 1
[0092] 1. Preparation of hydrophobic photothermal conversion materials
[0093] Weigh 1 mmol of the molar mass of cobalt acetate, nickel acetate tetrahydrate, copper acetate monohydrate, and manganese acetate. Then, add them to 150 ml of N, N-dimethylformamide and stir vigorously for 5 minutes with a magnetic stirrer. Subsequently, slowly add 5 mmol of terephthalic acid and continue to stir vigorously at room temperature for 2 hours. Finally, the final blue mixed solution is centrifuged at 8000 rpm for 2 minutes using a centrifuge, and washed three times with N, N-dimethylformamide. The collected blue precipitate is dried overnight in a vacuum oven at 60°C, and the dried product is finely ground to obtain the required high entropy alloy MOF precursor.
[0094] Next, the high entropy alloy MOF precursor material was transferred to a tube furnace, and the furnace temperature was raised to 700°C at a heating rate of 5°C per minute under the conditions of argon-hydrogen mixed gas (93% argon, 7% hydrogen) for calcination for 2 hours. When the temperature of the tube furnace dropped to room temperature, the calcined black powder was collected for subsequent operations.
[0095] Subsequently, 200 mg of the calcined black powder was weighed and added to 50 ml of a 5 mmol / L dilute sulfuric acid solution. Then, the mixed solution was ultrasonically treated for 5 min using an ultrasonic machine to make the material more evenly dispersed in the dilute sulfuric acid solution.
[0096] Then, the mixed solution and the beaker containing the solution were transferred to an oil bath pot and kept at 70°C for 6 hours to remove the impurities of non-high entropy alloy in the prepared material through the etching effect of sulfuric acid. Subsequently, the solution after the etching procedure was centrifuged using a centrifuge and washed 3 times with deionized water. The centrifuge parameters were set to 8000 revolutions per minute for 2 minutes. Finally, the collected black precipitate was freeze-dried using a freeze dryer to obtain the prepared CoNiCuMnAl@C material.
[0097] Finally, take 100 mg of the prepared CoNiCuMnAl@C material, add it to a wire-mouthed reagent bottle, and inject 100 ml of an ethanol solution containing 3 wt% hexadecyltrimethoxysilane. After tightening the bottle cap, place the reagent bottle in an ultrasonic machine and perform ultrasonic treatment for one hour to evenly disperse the material into the solution. During the ultrasonic process, the water in the ultrasonic machine needs to be replaced regularly to maintain a low temperature environment. After the treatment, transfer the wire-mouthed reagent bottle to room temperature (25°C) and let it stand for one hour. Finally, use a centrifuge to centrifuge the solution to obtain a precipitate, which is placed in an oven and kept warm at 110°C for 2 hours. After it cools down, the final hydrophobically modified photothermal conversion material (such as Figure 2 shown).
[0098] 2. Preparation of light absorbing layer
[0099] First, the aluminum sheet to be electrophoretically deposited needs to be pre-processed. The aluminum sheet with pre-customized specifications (90mm long, 56mm wide, 0.8mm thick, with a 4×4 circular hole matrix and a hole diameter of 2mm) will be laser-etched on the entire surface that needs electrophoretic deposition using a laser etching machine. Next, the etched aluminum sheet is placed in an ultrasonic machine for ultrasonic cleaning for one hour. After cleaning, the aluminum sheet is rinsed with anhydrous ethanol and deionized water, and dried after processing.
[0100] The process of preparing the electrophoretic deposition solution requires weighing 80 mg of hydrophobically modified photothermal conversion material, adding it to a wire mouth reagent bottle, and then injecting 100 ml of acetone solution. After tightening the bottle cap, put it into an ultrasonic machine for one hour of ultrasonic treatment. After treatment, add 13.5 mg of iodine to the solution, and then perform ultrasonic treatment for 3 minutes. The prepared electrophoretic deposition solution is placed in a pre-customized polytetrafluoroethylene electrophoretic deposition tank, and two beams are set at the notch, with a back-to-back distance of 1 cm. The aluminum sheet to be deposited is clamped on a beam and fixed with a negative electrode clamp of an adjustable power supply. On another beam, a piece of aluminum sheet that is also pretreated but not punched is clamped as the positive electrode, and the distance from the negative aluminum sheet is kept at about 1 cm. After the deposition starts, a 10V voltage is applied for deposition for 5 minutes. After stopping the deposition, a rubber-tipped dropper is used to blow air into the solution to stir it, so that the precipitated hydrophobically modified photothermal conversion material is suspended again, and the deposition process is repeated three times for a total of 15 minutes to form a photothermal conversion layer. The deposited aluminum sheet is cut into a predetermined shape.
[0101] Finally, the laser is used again to perform laser surface scanning etching (hydrophilic treatment) on the bottom surface of the aluminum sheet and the wall of the through hole, thus completing the preparation of the light absorption layer and using it for the subsequent step of salt evaporation and precipitation.
[0102] 3. Construction of evaporation device
[0103] The evaporation device is mainly composed of a light absorption layer, a water transfer layer and a heat insulation layer. In this embodiment, a 4×4 open-hole aluminum sheet deposited with a hydrophobic photothermal conversion material is used as a light absorption layer. The heat insulation layer (floating layer) adopts a polystyrene foam with heat insulation performance (0.04w / m / k) and capable of supporting floating, and is cut into a hexahedron with a length and width of 57mm and a height of 30mm. In order to divert the lower moisture upward, a water transfer hole with a diameter of about 20mm is dug in the middle of the square surface of the polystyrene foam, and runs through the entire hexahedron. In addition, absorbent cotton is selected as a water-conducting material to fill the voids of the polystyrene foam, and is spread between the photothermal layer and the polystyrene foam to form a water transfer layer. The hole is filled with about 1.8g of absorbent cotton, and 0.6g of absorbent cotton is filled between the photothermal layer and the polystyrene foam (water transfer layer).
[0104] Example 2
[0105] Compared with Example 1, except that the diameter of the through hole on the aluminum sheet is 3 mm, other conditions are the same as those in Example 1.
[0106] Example 3
[0107] Compared with Example 1, except that the diameter of the through hole on the aluminum sheet is 4 mm, other conditions are the same as those in Example 1.
[0108] Comparative Example 1
[0109] Compared with Example 2, except that the bottom surface of the aluminum sheet and the wall of the through hole are not subjected to hydrophilic treatment, the other conditions are the same as those of Example 2.
[0110] Performance Testing
[0111] 1. Evaporation test
[0112] The evaporation devices prepared in Examples 1 to 3 were tested respectively. 2 ) under the conditions of evaporation, the test results are as follows Figure 3 As shown. Figure 3 It can be found that as the aperture of the through hole on the aluminum sheet increases from 2mm to 3mm, the evaporation rate of the device increases significantly, but when the aperture is 4mm, the evaporation efficiency decreases. This shows that the size of the aperture on the directional salting-out interface evaporation device is better when the aperture is 3mm from the perspective of evaporation, and stable and long-lasting water evaporation performance can be achieved in the solar water evaporation system.
[0113] Furthermore, by recording the mass of evaporated water, it was found that the evaporation rate of the directional salting-out interface evaporation device increased steadily over time. Under stable illumination for about 3 hours, the evaporation rate of the evaporation device (aperture 3mm) reached 0.65kg / m 2 *h, In addition, under the same conditions, the evaporation rate of water is 0.36kg / m 2 *h. It can be seen that the evaporation rate of the evaporation device (aperture 3mm) is 1.8 times that of water, which shows that the evaporation device has good evaporation performance and salt collection performance.
[0114] The evaporation devices prepared in Example 2 and Comparative Example 1 were tested respectively. 2 ) under the conditions of evaporation, the test results are as follows Figure 4 As shown. Figure 4 It can be found that the evaporation amount of the evaporation device after laser hydrophilization treatment (Example 2) is much greater than the evaporation amount of the evaporation device without laser treatment (Comparative Example 1) (0.43 kg / m 2 *h). The reason for this phenomenon is that the more hydrophilic bottom surface is more conducive to the movement of water on its surface, increasing the contact between water and the light-to-heat conversion layer and the transfer of heat to the aqueous solution, thereby significantly increasing the evaporation amount.
[0115] 2. Salting out test
[0116] The evaporation devices prepared in Examples 1 to 3 were tested respectively. 2 ) under the conditions of salt analysis, the test results are as follows Figures 5 to 10As shown. It can be seen that when the through-hole aperture is 2mm, the through-holes on the evaporation device are basically covered by salt when the test is carried out for 60 minutes, and the precipitation of salt does not change significantly with the increase of the test time; while around the aluminum sheet, after 180 minutes, compared with the evaporation devices with 3mm and 4mm apertures, obvious salt precipitation growth appeared. This shows that when the through-hole aperture is selected as 2mm, the directional precipitation growth of salt is not conducive to the directional precipitation growth of salt due to the small aperture. Although there is obvious directional precipitation and growth of salt from the holes in both 3mm and 4mm, the evaporation amount of the photothermal conversion layer with an aperture of 4mm is less than that of the photothermal conversion layer with an aperture of 3mm. This is because the excessively large aperture will cause a reduction in the effective photothermal conversion area.
[0117] In summary, the evaporation device and preparation method provided by the present invention can significantly improve the evaporation efficiency of the evaporation device by providing a plurality of through holes penetrating the top and bottom surfaces of the thermally conductive substrate, performing hydrophilic treatment on the bottom surface of the thermally conductive substrate and the hole walls of the through holes, so that the hydrophobic photothermal conversion layer covers the top surface of the thermally conductive substrate, and can realize the directional precipitation of salt crystals at the through holes, thereby avoiding salt precipitation on the photothermal conversion layer and affecting the photothermal conversion efficiency of the photothermal conversion layer.
[0118] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered exemplary and non-limiting in all respects, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations falling within the meaning and scope of the equivalent elements of the claims be included in the invention. Any reference numeral in a claim should not be considered as limiting the claim to which it relates.
[0119] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.
Claims
1. An evaporation device, characterized in that: include: A heat-conducting substrate, on which a plurality of through holes penetrating the top and bottom surfaces of the heat-conducting substrate are provided, and the bottom surface of the heat-conducting substrate and the hole walls of the through holes are subjected to hydrophilic treatment; The hydrophobic light-to-heat conversion layer covers the top surface of the thermally conductive substrate.
2. The evaporation device according to claim 1, characterized in that: The hydrophobic photothermal conversion layer includes a hydrophobically modified photothermal conversion material, and the photothermal conversion material includes CoNiCuMnAl@C.
3. The evaporation device according to claim 1, characterized in that: The water contact angle of the hydrophobic light-to-heat conversion layer is greater than 90°; and / or the water contact angle of the bottom surface of the thermally conductive substrate and the hole wall of the through hole after hydrophilic treatment is less than 30°.
4. The evaporation device according to claim 1, characterized in that: The thickness of the thermally conductive substrate is 0.5-1 mm; and / or the diameter of the through hole is 2-5 mm.
5. The evaporation device according to claim 1, characterized in that: A water transfer layer is provided on the bottom surface of the heat-conducting substrate, and the water transfer layer is made of a water-conducting material.
6. The evaporation device according to claim 5, characterized in that: The bottom surface of the water transfer layer is provided with a heat insulation layer, and the heat insulation layer is provided with a water transfer hole penetrating the top and bottom surfaces of the heat insulation layer. The water transfer hole is filled with a water conductive filler, and the water conductive filler is in contact with the water transfer layer.
7. A method for preparing an evaporation device, characterized in that: include: A thermally conductive substrate and a photothermal conversion material are prepared, wherein the thermally conductive substrate is provided with a plurality of through holes penetrating the top and bottom surfaces thereof; Performing hydrophobic modification on photothermal conversion materials; depositing the hydrophobically modified photothermal conversion material on the top surface of the thermally conductive substrate; The bottom surface of the thermally conductive substrate and the hole walls of the through holes are subjected to hydrophilic treatment.
8. The method for preparing an evaporation device according to claim 7, characterized in that: The preparation method of the thermal conductive substrate includes: The top surface of the thermal conductive substrate is scanned and engraved using a laser, so that a micron-scale groove structure is formed on the top surface of the thermal conductive substrate; After scanning and engraving, the thermal conductive substrate is cleaned and dried.
9. The method for preparing an evaporation device according to claim 7, characterized in that: The preparation methods of photothermal conversion materials include: Weigh cobalt acetate, nickel acetate tetrahydrate, copper acetate monohydrate, and manganese acetate, add them into N,N-dimethylformamide, and stir evenly to obtain a mixed solution A; Add terephthalic acid to mixed solution A and stir vigorously for 1 to 3 hours to obtain mixed solution B; Centrifuging the mixed solution B to obtain a precipitate; The precipitate was washed by centrifugation using N,N-dimethylformamide, and the precipitate was collected and vacuum dried; Grinding the dried precipitate into powder to obtain a high entropy alloy MOF precursor; The high entropy alloy MOF precursor material is transferred to a tubular furnace, and under the condition of argon-hydrogen mixed gas, the furnace temperature is raised to 680-720°C at a heating rate of 5°C per minute, and after calcination for 1-2 hours, the temperature is lowered to room temperature to obtain a calcined black powder; The calcined black powder is added into a dilute sulfuric acid solution with a concentration of 3 to 6 mmol / L, and ultrasonically dispersed to obtain a mixed solution C; The mixed solution C is placed in an environment of 60-80°C, and the impurities in the black powder are etched by sulfuric acid; After etching is completed, the mixed solution C is centrifuged, and the black precipitate is collected, washed, and dried to obtain the CoNiCuMnAl@C photothermal conversion material.
10. The method for preparing an evaporation device according to claim 7, characterized in that: The hydrophilic treatment methods for the bottom surface of the thermal conductive substrate and the hole wall of the through hole include: The bottom surface of the thermal conductive substrate and the hole wall of the through hole are scanned and engraved by laser.
Citation Information
Patent Citations
Photo-thermal conversion seawater desalination device, manufacturing method thereof, and seawater desalination method
CN113479958A
Composite membrane material, preparation method thereof and solar evaporator
CN115746383A
Preparation method of six-element high-entropy monatomic nitrogen-rich porous photo-thermal material
CN117843065A
Systems and methods for photothermal material
US20200041169A1
Composite membrane for a membrane distillation system
US4419242A