Preparation method of self-cleaning water treatment filler

By preparing a zinc ferrite-alumina composite coating on stainless steel Pall rings, the problem of low treatment efficiency of highly toxic organic pollutants in existing technologies is solved, and the efficient photocatalytic degradation capability of self-cleaning water treatment fillers is realized.

CN118908405AActive Publication Date: 2024-11-08SHENYANG LIGONG UNIV
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411339124.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-25
Publication Date
2024-11-08
Estimated Expiration
2044-09-25

AI Technical Summary

Technical Problem

Existing technologies are difficult to effectively treat highly toxic organic pollutants, affecting the efficiency of biochemical treatment, and there are challenges in the preparation of water treatment packing materials for photocatalytic oxidation technology.

Method used

A zinc ferrite-alumina composite coating was prepared on a stainless steel Pall ring. A dense and uniform coating was formed by acid washing, electrode reaction and sol-gel method, which improved the photocatalytic activity of the filler.

Benefits of technology

Self-cleaning water treatment packing rapidly degrades organic pollutants under light, has continuous treatment capabilities, and is suitable for the purification of various organic pollutants.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to a preparation method of a self-cleaning water treatment filler, and belongs to the field of environmental pollution purification materials. The method comprises the following steps: pickling a stainless steel Pall ring, carrying out an electrode reaction on the pickled stainless steel Pall ring to generate a zinc ferrite film, and finally immersing the zinc ferrite film coated stainless steel Pall ring into a solution to obtain a Pall ring with a zinc ferrite-aluminum oxide composite coating, namely the self-cleaning water treatment filler. The zinc ferrite-aluminum oxide composite coating is prepared on the stainless steel Pall ring through scientific design and optimization of raw materials and a preparation process, and the relative mass percentage content of zinc ferrite-aluminum oxide in the coating is scientifically optimized, so that the self-cleaning water treatment filler has ideal activity of purifying organic pollutants, and the service life of the filler is prolonged. And the method can be widely applied to the treatment process of various organic pollutants in water.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of environmental pollution purification materials, and in particular relates to a method for preparing a self-cleaning water treatment filler. Background Art

[0002] Organic pollutants exist in large quantities in industrial and domestic wastewater. There are many types of organic pollutants and they pose a huge threat to the natural environment and human health. Wastewater contaminated by such pollutants must undergo deep treatment before it can be discharged into natural water bodies.

[0003] In the process of biochemical treatment of organic pollutants, fillers are used. Fillers can intercept pollutants in wastewater, and use microorganisms attached to the fillers to decompose and purify the intercepted organic pollutants. Since some organic pollutants are highly toxic, they directly affect the efficiency of biochemical treatment and need to be treated by other methods.

[0004] Photocatalytic oxidation technology is widely used in the treatment of organic pollutants in the environment. Photocatalytic oxidation can degrade a variety of organic pollutants. This method can replace the role of microorganisms in biochemical treatment. The preparation of water treatment fillers with photocatalytic purification activity is a technical problem that needs to be solved urgently. Summary of the invention

[0005] In view of the problems existing in the prior art, the present invention aims to provide a method for preparing a self-cleaning water treatment filler, which can be used for purifying organic pollutants in water.

[0006] A method for preparing a self-cleaning water treatment filler comprises the following process steps:

[0007] Step 1: Pickling of stainless steel ball ring

[0008] (1) Immerse the stainless steel ball ring in a 0.2 mol / L hydrochloric acid solution for 50 min to remove impurities on the stainless steel ball ring;

[0009] (2) washing the stainless steel ball ring treated as above with pure water, and drying at 80° C. for 2 h to obtain an acid-washed stainless steel ball ring;

[0010] Step 2: Electrode reaction to form zinc ferrite film

[0011] (1) Add 320-360 mL of pure water, 20-23 mL of acetic acid, 10-12 g of disodium ethylenediaminetetraacetate, and 15-17 g of zinc chloride into a beaker and stir to form solution A;

[0012] (2) Connect the anode of a 12 V power supply to a stainless steel ball ring and the cathode to a titanium plate. Immerse the two electrodes in solution A, control the current between the two electrodes to 1.8 A, and conduct the reaction for 15 min.

[0013] (3) The stainless steel ball ring after the electrode reaction is washed with pure water, dried at 80° C. for 2 h, and then calcined at 260-280° C. for 1 h to obtain a stainless steel ball ring coated with a zinc ferrite film;

[0014] Step 3: Sol-gel coating of aluminum oxide film

[0015] (1) Add 4.5-5.3 g of emulsifier OP-10, 7.2-8.3 g of aluminum isopropoxide, and 2.7-3.1 g of dodecyltrimethylammonium bromide to 120-130 mL of ethanol and stir to form solution B;

[0016] (2) Add 1.1-1.2 mL of concentrated hydrochloric acid to 18-21 mL of pure water and stir to form solution C;

[0017] (3) Add solution C to solution B and stir to form solution D. Immerse the zinc ferrite film-coated stainless steel ball ring in solution D for 5 minutes, then take it out and let it stand for 20 minutes.

[0018] (4) The ball ring after the above treatment is dried at 90° C. for 8 hours, and then calcined at 335-360° C. for 3 hours to obtain a ball ring with a zinc ferrite-aluminum oxide composite coating, which is a self-cleaning water treatment filler.

[0019] The stainless steel ball ring is punched from a metal sheet, and two rows of window holes with inwardly extending tongues are opened on the ring wall, with a specification of 25mm×25mm×0.6mm. The specific surface area of ​​the stainless steel ball ring is 219m 2 / m 3 , porosity 0.93m 3 / m 3 .

[0020] A self-cleaning water treatment filler, prepared by the above method, wherein the self-cleaning water treatment filler has a specific surface area of ​​252 to 263 m 2 / m 3 , porosity 0.85~0.88m 3 / m 3 .

[0021] The total mass percentage of the zinc ferrite-aluminum oxide composite coating in the self-cleaning water treatment filler is 3.0% to 3.3%, of which the zinc ferrite accounts for 1.5% to 1.7% and the aluminum oxide accounts for 1.5% to 1.6%.

[0022] The various chemical raw materials are all pure materials.

[0023] Compared with the prior art, the advantages of the present invention are:

[0024] (1) The present invention prepares a zinc ferrite-aluminum oxide composite coating on a stainless steel ball ring by scientifically designing and optimizing raw materials and preparation processes. The relative mass percentage of zinc ferrite-aluminum oxide in the coating is scientifically optimized so that the self-cleaning water treatment filler has an ideal activity for purifying organic pollutants.

[0025] (2) The zinc ferrite-aluminum oxide composite coating has a strong bonding force with the stainless steel ball ring, the coating is dense and evenly distributed, has strong mechanical strength, and has ideal corrosion resistance.

[0026] (3) The self-cleaning water treatment filler can quickly degrade organic pollutants under light, has the ability to continuously treat organic pollutants in water, and can be widely used in the treatment process of various organic pollutants in water. DETAILED DESCRIPTION

[0027] In order to further understand the present invention, the present invention is further described in detail below in conjunction with embodiments.

[0028] All chemical raw materials in the examples are pure materials.

[0029] Example 1

[0030] A method for preparing a self-cleaning water treatment filler comprises the following process steps:

[0031] Step 1: Pickling of stainless steel ball ring

[0032] (1) Immerse the stainless steel ball ring in a 0.2 mol / L hydrochloric acid solution for 50 min to remove impurities on the stainless steel ball ring;

[0033] (2) The stainless steel ball ring treated as above is washed with pure water and dried at 80° C. for 2 h to obtain an acid-washed stainless steel ball ring.

[0034] Step 2: Electrode reaction to form zinc ferrite film

[0035] (1) Add 320 mL of pure water, 20 mL of acetic acid, 10 g of disodium ethylenediaminetetraacetate, and 15 g of zinc chloride into a beaker and stir to form solution A;

[0036] (2) Connect the anode of a 12 V power supply to a stainless steel ball ring and the cathode to a titanium plate. Immerse the two electrodes in solution A, control the current between the two electrodes to 1.8 A, and conduct the reaction for 15 min.

[0037] (3) The stainless steel ball ring after the electrode reaction was washed with pure water, dried at 80° C. for 2 h, and then calcined at 260° C. for 1 h to obtain a stainless steel ball ring coated with a zinc ferrite film.

[0038] Step 3: Sol-gel coating of aluminum oxide film

[0039] (1) Add 4.5 g of emulsifier OP-10, 7.2 g of aluminum isopropoxide, and 2.7 g of dodecyltrimethylammonium bromide to 120 mL of ethanol and stir to form solution B;

[0040] (2) Add 1.1 mL of concentrated hydrochloric acid to 18 mL of pure water and stir to form solution C;

[0041] (3) Add solution C to solution B and stir to form solution D. Immerse the zinc ferrite film-coated stainless steel ball ring in solution D for 5 minutes, then take it out and let it stand for 20 minutes.

[0042] (4) The ball ring after the above treatment is dried at 90° C. for 8 hours, and then calcined at 335° C. for 3 hours to obtain a ball ring coated with an aluminum oxide film, which is a self-cleaning water treatment filler.

[0043] The total mass percentage of the zinc ferrite-aluminum oxide composite coating in the self-cleaning water treatment filler is 3.0%, of which the zinc ferrite accounts for 1.5% and the aluminum oxide accounts for 1.5%.

[0044] Example 2

[0045] A method for preparing a self-cleaning water treatment filler comprises the following process steps:

[0046] Step 1: Pickling of stainless steel ball ring

[0047] (1) Immerse the stainless steel ball ring in a 0.2 mol / L hydrochloric acid solution for 50 min to remove impurities on the stainless steel ball ring;

[0048] (2) The stainless steel ball ring treated as above is washed with pure water and dried at 80° C. for 2 h to obtain an acid-washed stainless steel ball ring.

[0049] Step 2: Electrode reaction to form zinc ferrite film

[0050] (1) Add 330 mL of pure water, 21 mL of acetic acid, 10 g of disodium ethylenediaminetetraacetate, and 15.5 g of zinc chloride into a beaker and stir to form solution A;

[0051] (2) Connect the anode of a 12 V power supply to a stainless steel ball ring and the cathode to a titanium plate. Immerse the two electrodes in solution A, control the current between the two electrodes to 1.8 A, and conduct the reaction for 15 min.

[0052] (3) The stainless steel ball ring after the electrode reaction was washed with pure water, dried at 80° C. for 2 h, and then calcined at 265° C. for 1 h to obtain a stainless steel ball ring coated with a zinc ferrite film.

[0053] Step 3: Sol-gel coating of aluminum oxide film

[0054] (1) Add 4.7 g of emulsifier OP-10, 7.4 g of aluminum isopropoxide, and 2.8 g of dodecyltrimethylammonium bromide to 123 mL of ethanol and stir to form solution B;

[0055] (2) Add 1.1 mL of concentrated hydrochloric acid to 18 mL of pure water and stir to form solution C;

[0056] (3) Add solution C to solution B and stir to form solution D. Immerse the zinc ferrite film-coated stainless steel ball ring in solution D for 5 minutes, then take it out and let it stand for 20 minutes.

[0057] (4) The ball ring after the above treatment is dried at 90° C. for 8 hours, and then calcined at 340° C. for 3 hours to obtain a ball ring coated with an aluminum oxide film, which is a self-cleaning water treatment filler.

[0058] The total mass percentage of the zinc ferrite-aluminum oxide composite coating in the self-cleaning water treatment filler is 3.1%, of which the zinc ferrite accounts for 1.6% and the aluminum oxide accounts for 1.5%.

[0059] Example 3

[0060] A method for preparing a self-cleaning water treatment filler comprises the following process steps:

[0061] Step 1: Pickling of stainless steel ball ring

[0062] (1) Immerse the stainless steel ball ring in a 0.2 mol / L hydrochloric acid solution for 50 min to remove impurities on the stainless steel ball ring;

[0063] (2) The stainless steel ball ring treated as above is washed with pure water and dried at 80° C. for 2 h to obtain an acid-washed stainless steel ball ring.

[0064] Step 2: Electrode reaction to form zinc ferrite film

[0065] (1) Add 340 mL of pure water, 21 mL of acetic acid, 11 g of disodium ethylenediaminetetraacetate, and 16 g of zinc chloride into a beaker and stir to form solution A;

[0066] (2) Connect the anode of a 12 V power supply to a stainless steel ball ring and the cathode to a titanium plate. Immerse the two electrodes in solution A, control the current between the two electrodes to 1.8 A, and conduct the reaction for 15 min.

[0067] (3) The stainless steel ball ring after the electrode reaction was washed with pure water, dried at 80° C. for 2 h, and then calcined at 270° C. for 1 h to obtain a stainless steel ball ring coated with a zinc ferrite film.

[0068] Step 3: Sol-gel coating of aluminum oxide film

[0069] (1) Add 4.9 g of emulsifier OP-10, 7.8 g of aluminum isopropoxide, and 2.9 g of dodecyltrimethylammonium bromide to 125 mL of ethanol and stir to form solution B;

[0070] (2) Add 1.1 mL of concentrated hydrochloric acid to 19 mL of pure water and stir to form solution C;

[0071] (3) Add solution C to solution B and stir to form solution D. Immerse the zinc ferrite film-coated stainless steel ball ring in solution D for 5 minutes, then take it out and let it stand for 20 minutes.

[0072] (4) The ball ring after the above treatment is dried at 90° C. for 8 hours, and then calcined at 345° C. for 3 hours to obtain a ball ring coated with an aluminum oxide film, which is a self-cleaning water treatment filler.

[0073] The total mass percentage of the zinc ferrite-aluminum oxide composite coating in the self-cleaning water treatment filler is 3.1%, of which the zinc ferrite accounts for 1.6% and the aluminum oxide accounts for 1.5%.

[0074] Example 4

[0075] A method for preparing a self-cleaning water treatment filler comprises the following process steps:

[0076] Step 1: Pickling of stainless steel ball ring

[0077] (1) Immerse the stainless steel ball ring in a 0.2 mol / L hydrochloric acid solution for 50 min to remove impurities on the stainless steel ball ring;

[0078] (2) The stainless steel ball ring treated as above is washed with pure water and dried at 80° C. for 2 h to obtain an acid-washed stainless steel ball ring.

[0079] Step 2: Electrode reaction to form zinc ferrite film

[0080] (1) Add 350 mL of pure water, 22 mL of acetic acid, 11 g of disodium ethylenediaminetetraacetate, and 16 g of zinc chloride into a beaker and stir to form solution A;

[0081] (2) Connect the anode of a 12 V power supply to a stainless steel ball ring and the cathode to a titanium plate. Immerse the two electrodes in solution A, control the current between the two electrodes to 1.8 A, and conduct the reaction for 15 min.

[0082] (3) The stainless steel ball ring after the electrode reaction was washed with pure water, dried at 80° C. for 2 h, and then calcined at 275° C. for 1 h to obtain a zinc ferrite film-coated stainless steel ball ring.

[0083] Step 3: Sol-gel coating of aluminum oxide film

[0084] (1) Add 5.1 g of emulsifier OP-10, 8.0 g of aluminum isopropoxide, and 3.0 g of dodecyltrimethylammonium bromide to 128 mL of ethanol and stir to form solution B;

[0085] (2) Add 1.2 mL of concentrated hydrochloric acid to 20 mL of pure water and stir to form solution C;

[0086] (3) Add solution C to solution B and stir to form solution D. Immerse the zinc ferrite film-coated stainless steel ball ring in solution D for 5 minutes, then take it out and let it stand for 20 minutes.

[0087] (4) The ball ring after the above treatment is dried at 90° C. for 8 hours, and then calcined at 355° C. for 3 hours to obtain a ball ring coated with an aluminum oxide film, which is a self-cleaning water treatment filler.

[0088] The total mass percentage of the zinc ferrite-aluminum oxide composite coating in the self-cleaning water treatment filler is 3.2%, of which the zinc ferrite accounts for 1.6% and the aluminum oxide accounts for 1.6%.

[0089] Example 5

[0090] A method for preparing a self-cleaning water treatment filler comprises the following process steps:

[0091] Step 1: Pickling of stainless steel ball ring

[0092] (1) Immerse the stainless steel ball ring in a 0.2 mol / L hydrochloric acid solution for 50 min to remove impurities on the stainless steel ball ring;

[0093] (2) The stainless steel ball ring treated as above is washed with pure water and dried at 80° C. for 2 h to obtain an acid-washed stainless steel ball ring.

[0094] Step 2: Electrode reaction to form zinc ferrite film

[0095] (1) Add 360 mL of pure water, 23 mL of acetic acid, 12 g of disodium ethylenediaminetetraacetate, and 17 g of zinc chloride into a beaker and stir to form solution A;

[0096] (2) Connect the anode of a 12 V power supply to a stainless steel ball ring and the cathode to a titanium plate. Immerse the two electrodes in solution A, control the current between the two electrodes to 1.8 A, and conduct the reaction for 15 min.

[0097] (3) The stainless steel ball ring after the electrode reaction was washed with pure water, dried at 80° C. for 2 h, and then calcined at 280° C. for 1 h to obtain a stainless steel ball ring coated with a zinc ferrite film.

[0098] Step 3: Sol-gel coating of aluminum oxide film

[0099] (1) Add 5.3 g of emulsifier OP-10, 8.3 g of aluminum isopropoxide, and 3.1 g of dodecyltrimethylammonium bromide to 130 mL of ethanol and stir to form solution B;

[0100] (2) Add 1.2 mL of concentrated hydrochloric acid to 21 mL of pure water and stir to form solution C;

[0101] (3) Add solution C to solution B and stir to form solution D. Immerse the zinc ferrite film-coated stainless steel ball ring in solution D for 5 minutes, then take it out and let it stand for 20 minutes.

[0102] (4) The ball ring after the above treatment is dried at 90° C. for 8 hours, and then calcined at 360° C. for 3 hours to obtain a ball ring coated with an aluminum oxide film, which is a self-cleaning water treatment filler.

[0103] The total mass percentage of the zinc ferrite-aluminum oxide composite coating in the self-cleaning water treatment filler is 3.3%, of which the zinc ferrite accounts for 1.7% and the aluminum oxide accounts for 1.6%.

Claims

1. A method for preparing a self-cleaning water treatment filler, characterized in that: The process includes the following steps: Step 1: Pickling of stainless steel ball ring (1) Immerse the stainless steel ball ring in a 0.2 mol / L hydrochloric acid solution for 50 min to remove impurities on the stainless steel ball ring; (2) washing the stainless steel ball ring treated as above with pure water, and drying at 80° C. for 2 h to obtain an acid-washed stainless steel ball ring; Step 2: Electrode reaction to form zinc ferrite film (1) Add 320-360 mL of pure water, 20-23 mL of acetic acid, 10-12 g of disodium ethylenediaminetetraacetate, and 15-17 g of zinc chloride into a beaker and stir to form solution A; (2) Connect the anode of a 12 V power supply to a stainless steel ball ring and the cathode to a titanium plate. Immerse the two electrodes in solution A, control the current between the two electrodes to 1.8 A, and conduct the reaction for 15 min. (3) The stainless steel ball ring after the electrode reaction is washed with pure water, dried at 80° C. for 2 h, and then calcined at 260-280° C. for 1 h to obtain a stainless steel ball ring coated with a zinc ferrite film; Step 3: Sol-gel coating of aluminum oxide film (1) Add 4.5-5.3 g of emulsifier OP-10, 7.2-8.3 g of aluminum isopropoxide, and 2.7-3.1 g of dodecyltrimethylammonium bromide to 120-130 mL of ethanol and stir to form solution B; (2) Add 1.1-1.2 mL of concentrated hydrochloric acid to 18-21 mL of pure water and stir to form solution C; (3) Add solution C to solution B and stir to form solution D. Immerse the zinc ferrite film-coated stainless steel ball ring in solution D for 5 minutes, then take it out and let it stand for 20 minutes. (4) The ball ring after the above treatment is dried at 90° C. for 8 hours, and then calcined at 335-360° C. for 3 hours to obtain a ball ring with a zinc ferrite-aluminum oxide composite coating, which is a self-cleaning water treatment filler.

2. The method for preparing a self-cleaning water treatment filler according to claim 1, characterized in that: The stainless steel ball ring is punched from a metal sheet, and two rows of window holes with inwardly extending tongues are opened on the ring wall, with a specification of 25mm×25mm×0.6mm. The specific surface area of ​​the stainless steel ball ring is 219m 2 / m 3 , porosity 0.93m 3 / m 3 .

3. A self-cleaning water treatment filler, prepared by the method according to claim 1 or 2, characterized in that: The specific surface area of ​​the self-cleaning water treatment filler is 252-263m 2 / m 3 , porosity 0.85~0.88m 3 / m 3 .

4. A self-cleaning water treatment filler according to claim 3, characterized in that: The total mass percentage of the zinc ferrite-aluminum oxide composite coating in the self-cleaning water treatment filler is 3.0% to 3.3%, of which the zinc ferrite accounts for 1.5% to 1.7% and the aluminum oxide accounts for 1.5% to 1.6%.

Citation Information

Patent Citations

  • Preparation method and application thereof for zinc ferrite / titanium dioxide nano compounded visible light photocatalyst

    CN101653728A

  • Zinc ferrite-cobalt ferrite heterojunction composite catalyst as well as preparation method and application thereof

    CN108855105A

  • Preparation method of self-cleaning fibers

    CN109382089A

  • Novel biological membrane wastewater treatment

    CN1122779A

  • Anti-compaction loofah sponge composite filler as well as preparation method and application thereof

    CN114247417A