Germanate red-light perovskite quantum dot glass with high luminous efficiency and preparation method thereof
By adding Nb5+ to germanate glass and annealing and heat treatment, a high luminous efficiency germanate red light perovskite quantum dot glass is prepared, solving the photoelectric performance and stability of traditional perovskite quantum dot glass. The disadvantages of this method achieve excellent optical performance and good thermal stability.
Patent Information
- Application Number
- CN202410972749.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-19
AI Technical Summary
Traditional CsPbBrI2 perovskite quantum dot glasses are difficult to meet modern technical requirements in terms of photoelectric performance and stability, especially in terms of improvements in thermal stability and optical performance.
By mixing H3BO3, GeO2, ZnO, CaO, Cs2CO3, PbO, NaI, NbBr and Nb2O5, melting, annealing and heat treatment, a high luminescence efficiency germanate red light perovskite quantum dot glass was prepared, and Nb5+ was incorporated into Nb5+ To improve fluorescent quantum yield and remove internal stress by annealing and heat treatment, the stability and thermal stability of the glass are enhanced.
The germanate red light perovskite quantum dot glass has excellent optical performance and good thermal stability, high fluorescence quantum yield, excellent luminescence characteristics and good temperature rebound.
Smart Images

Figure CN118908568A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of solid luminescent materials, and in particular to a high-luminescent-efficiency germanate red-light perovskite quantum dot glass and a preparation method thereof. Background Art
[0002] In recent years, all-inorganic perovskite quantum dots have the advantages of adjustable emission peak position, narrow emission spectrum, high fluorescence quantum efficiency, convenient preparation, and strong defect tolerance. Therefore, they are widely used in optoelectronic devices such as solar cells, light-emitting diodes and lasers. However, due to their inherent crystal structure, ion exchange of surface ligands, and abnormal sensitivity to environmental factors such as light, water, oxygen and heat, stability issues restrict their application. Oxide glass materials have the advantages of dense network structure, high stability and easy preparation. Encapsulating perovskite quantum dots in inorganic glass materials has become an effective means to improve the stability of perovskite quantum dots. Even though CsPbBrI2 perovskite quantum dots have been applied to various fields, their optoelectronic properties and stability are still difficult to meet technical requirements. With the advancement of science and technology, various fields have put forward higher requirements for the optoelectronic properties and stability of CsPbBrI2 perovskite quantum dots, and traditional CsPbBrI2 perovskite quantum dot glass has gradually failed to meet the requirements.
[0003] Therefore, how to improve the photoelectric performance and stability of CsPbBrI2 perovskite quantum dots has become a technical problem that needs to be urgently solved in this field. Summary of the invention
[0004] The object of the present invention is to provide a high-luminous efficiency germanate red light perovskite quantum dot glass and a preparation method thereof. The germanate red light perovskite quantum dot glass prepared by the preparation method provided by the present invention has not only excellent optical properties but also good thermal stability.
[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0006] The present invention provides a method for preparing a germanate red light perovskite quantum dot glass with high luminous efficiency, comprising the following steps:
[0007] (1) H3BO3, GeO2, ZnO, CaO, Cs2CO3, PbO, NaI, NbBr and Nb2O5 are mixed and melted to obtain a glass melt;
[0008] (2) annealing the glass melt obtained in step (1) to obtain a glass block;
[0009] (3) heat-treating the glass block obtained in step (2) to obtain a germanate red light perovskite quantum dot glass with high luminous efficiency.
[0010] Preferably, in step (1), the molar ratio of H3BO3, GeO2, ZnO, CaO, Cs2CO3, PbO, NaI, NbBr and Nb2O5 is (35-55): (25-40): (4-6): (3-5): (4-6): (2.5-3): 2: 4: (0.7-3.5).
[0011] Preferably, the molar ratio of H3BO3, GeO2, ZnO, CaO, Cs2CO3, PbO, NaI, NbBr and Nb2O5 is 40:40:4:3:4.5:2.5:2:4:(0.7-3.5).
[0012] Preferably, the melting and holding temperature in step (1) is 900-1050° C., and the melting and holding time is 10-40 minutes.
[0013] Preferably, the melting holding temperature is 1000° C., and the melting holding time is 20 minutes.
[0014] Preferably, the holding temperature of the annealing treatment in step (2) is 300-400° C., and the holding time of the annealing treatment is 2-5 hours.
[0015] Preferably, the holding temperature of the annealing treatment is 350° C., and the holding time of the annealing treatment is 3 hours.
[0016] Preferably, the holding temperature of the heat treatment in step (3) is 500-550° C., and the holding time of the heat treatment is 3-6 hours.
[0017] Preferably, the heat treatment is carried out at a holding temperature of 520° C. and for a holding time of 4 hours.
[0018] The present invention provides a germanate red light perovskite quantum dot glass with high luminous efficiency prepared by the preparation method described in the above technical solution.
[0019] The present invention provides a method for preparing a germanate red light perovskite quantum dot glass with high luminous efficiency, comprising the following steps: (1) mixing H3BO3, GeO2, ZnO, CaO, Cs2CO3, PbO, NaI, NbBr and Nb2O5 and melting them to obtain a glass melt; (2) annealing the glass melt obtained in step (1) to obtain a glass block; (3) heat-treating the glass block obtained in step (2) to obtain a germanate red light perovskite quantum dot glass with high luminous efficiency. The present invention prepares a germanate red light perovskite quantum dot glass with high luminous efficiency by doping Nb in the germanate red light perovskite quantum dot glass. 5+, which can effectively improve the fluorescence quantum yield of the glass, thereby improving its optical properties; by annealing the glass melt, the internal stress generated by the glass during the cooling process can be removed, thereby improving the stability of the glass; finally, the thermal stability of the germanium glass can be further improved by heat treatment, thereby obtaining a germanate red light perovskite quantum dot glass with excellent optical properties and good thermal stability. The results of the examples show that the germanate red light perovskite quantum dot glass provided by the present invention not only has excellent optical properties, but also has good thermal stability. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 XRD diagram of the germanate red light perovskite quantum dot glass obtained in Examples 1 to 5 and Comparative Example 1;
[0021] Figure 2 This is a TEM image of the germanate red light perovskite quantum dot glass obtained in Example 3;
[0022] Figure 3 This is a size distribution histogram of the germanate red light perovskite quantum dot glass obtained in Example 3;
[0023] Figure 4 This is the HTEM image of the germanate red light perovskite quantum dot glass obtained in Example 3;
[0024] Figure 5 The emission spectra of the germanate red light perovskite quantum dot glass obtained in Examples 1 to 5 and Comparative Example 1;
[0025] Figure 6 This is the FTIR image of the germanate red light perovskite quantum dot glass obtained in Example 3;
[0026] Figure 7 This is the Raman spectrum of the germanate red light perovskite quantum dot glass obtained in Example 3;
[0027] Figure 8 This is the heating spectrum of the germanate red light perovskite quantum dot glass obtained in Example 3;
[0028] Fig. 9 This is the cooling spectrum of the germanate red light perovskite quantum dot glass obtained in Example 3;
[0029] Fig.10 This is the luminescence intensity variation curve of the germanate red light perovskite quantum dot glass obtained in Example 3 during the heating and cooling processes. DETAILED DESCRIPTION
[0030] The present invention provides a method for preparing a germanate red light perovskite quantum dot glass with high luminous efficiency, comprising the following steps:
[0031] (1) H3BO3, GeO2, ZnO, CaO, Cs2CO3, PbO, NaI, NbBr and Nb2O5 are mixed and melted to obtain a glass melt;
[0032] (2) annealing the glass melt obtained in step (1) to obtain a glass block;
[0033] (3) heat-treating the glass block obtained in step (2) to obtain a germanate red light perovskite quantum dot glass with high luminous efficiency.
[0034] The present invention mixes H3BO3, GeO2, ZnO, CaO, Cs2CO3, PbO, NaI, NbBr and Nb2O5 and melts them to obtain a glass melt.
[0035] In the present invention, unless otherwise specified, the raw materials used are commercially available products well known to those skilled in the art or products prepared using processes well known to those skilled in the art.
[0036] In the present invention, the molar ratio of H3BO3, GeO2, ZnO, CaO, Cs2CO3, PbO, NaI, NbBr and Nb2O5 is preferably (35-55): (25-40): (4-6): (3-5): (4-6): (2.5-3): 2: 4: (0.7-3.5), and more preferably 40: 40: 4: 3: 4.5: 2.5: 2: 4: (0.7-3.5). The present invention can further improve the optical properties and chemical stability of the glass by controlling the usage relationship of the raw materials.
[0037] The present invention has no particular limitation on the specific operation of the mixing, which can be determined according to the technical common sense of those skilled in the art.
[0038] In the present invention, the melting is preferably carried out in a muffle furnace. The present invention has no particular limitation on the specific model of the muffle furnace, and a commercially available muffle furnace well known to those skilled in the art can be used.
[0039] In the present invention, the melting holding temperature is preferably 900-1050°C, more preferably 1000°C; the melting holding time is preferably 10-40 minutes, more preferably 20 minutes. The present invention can ensure that the raw materials are completely melted to form a uniform glass melt by controlling the melting process parameters.
[0040] After obtaining the glass melt, the present invention performs annealing treatment on the glass melt to obtain a glass block.
[0041] In the present invention, the annealing treatment is preferably performed by pouring the molten glass onto a preheating plate and then transferring it to an annealing furnace for annealing. The present invention can avoid excessive internal stress caused by rapid cooling of the molten glass in air, which may cause cracking of the glass block.
[0042] In the present invention, the holding temperature of the annealing treatment is preferably 300-400° C., more preferably 350° C.; the holding time of the annealing treatment is preferably 2-5 hours, more preferably 3 hours. The present invention can eliminate the internal stress in the glass block through annealing treatment.
[0043] After obtaining the glass block, the present invention performs heat treatment on the glass block to obtain germanate red light perovskite quantum dot glass with high luminous efficiency.
[0044] In the present invention, the heat treatment holding temperature is preferably 500-550°C, more preferably 520°C; the heat treatment holding time is preferably 3-6h, more preferably 4h. The present invention can further improve the thermal stability of the germanate red light perovskite quantum dot glass through heat treatment.
[0045] The present invention involves doping Nb into the germanate red light perovskite quantum dot glass. 5+ , which can effectively improve the fluorescence quantum yield of the glass, thereby improving its optical properties; by annealing the glass melt, the internal stress generated by the glass during the cooling process can be removed, thereby improving the stability of the glass; finally, the thermal stability of the germanium glass can be further improved by heat treatment, thereby obtaining germanate red light perovskite quantum dot glass with excellent optical properties and good thermal stability.
[0046] The present invention provides a germanate red light perovskite quantum dot glass with high luminous efficiency prepared by the preparation method described in the above technical solution.
[0047] The germanate red light perovskite quantum dot glass provided by the present invention has high fluorescence quantum yield, excellent luminescence characteristics and good thermal stability.
[0048] The technical solutions in the present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0049] Example 1
[0050] A method for preparing a germanate red light perovskite quantum dot glass with high luminous efficiency, comprising the following steps:
[0051] (1) H3BO3, GeO2, ZnO, CaO, Cs2CO3, PbO, NaI, NbBr and Nb2O5 are mixed and melted in a muffle furnace to obtain a glass melt; the molar ratio of H3BO3, GeO2, ZnO, CaO, Cs2CO3, PbO, NaI, NbBr and Nb2O5 is 40:40:4:3:4.5:2.5:2:4:0.7; the melting holding temperature is 1000°C, and the melting holding time is 20 minutes;
[0052] (2) pouring the glass melt obtained in step (1) onto a preheating plate, and then transferring it to an annealing furnace for annealing to obtain a glass block; the annealing temperature is 350° C., and the annealing time is 3 hours;
[0053] (3) The glass block obtained in step (2) is heat-treated to obtain a germanate red light perovskite quantum dot glass with high luminous efficiency, which is denoted as PG1; the heat treatment is carried out at a holding temperature of 520° C. for a holding time of 4 h.
[0054] Example 2
[0055] A method for preparing a high-luminescence-efficiency germanate red-light perovskite quantum dot glass comprises the following steps:
[0056] (1) H3BO3, GeO2, ZnO, CaO, Cs2CO3, PbO, NaI, NbBr and Nb2O5 are mixed and melted in a muffle furnace to obtain a glass melt; the molar ratio of H3BO3, GeO2, ZnO, CaO, Cs2CO3, PbO, NaI, NbBr and Nb2O5 is 40:40:4:3:4.5:2.5:2:4:1.4; the melting holding temperature is 1000°C and the melting holding time is 20 minutes;
[0057] (2) pouring the glass melt obtained in step (1) onto a preheating plate, and then transferring it to an annealing furnace for annealing to obtain a glass block; the annealing temperature is 350° C., and the annealing time is 3 hours;
[0058] (3) The glass block obtained in step (2) is heat-treated to obtain a high-luminescence-efficiency germanate red-light perovskite quantum dot glass, which is denoted as PG2; the heat treatment is carried out at a holding temperature of 520° C. for a holding time of 4 h.
[0059] Example 3
[0060] A method for preparing a high-luminescence-efficiency germanate red-light perovskite quantum dot glass comprises the following steps:
[0061] (1) H3BO3, GeO2, ZnO, CaO, Cs2CO3, PbO, NaI, NbBr and Nb2O5 are mixed and melted in a muffle furnace to obtain a glass melt; the molar ratio of H3BO3, GeO2, ZnO, CaO, Cs2CO3, PbO, NaI, NbBr and Nb2O5 is 40:40:4:3:4.5:2.5:2:4:2.1; the melting holding temperature is 1000°C, and the melting holding time is 20 minutes;
[0062] (2) pouring the glass melt obtained in step (1) onto a preheating plate, and then transferring it to an annealing furnace for annealing to obtain a glass block; the annealing temperature is 350° C., and the annealing time is 3 hours;
[0063] (3) The glass block obtained in step (2) is heat-treated to obtain a high-luminescence-efficiency germanate red-light perovskite quantum dot glass, which is denoted as PG3; the heat treatment is carried out at a holding temperature of 520° C. for a holding time of 4 h.
[0064] Example 4
[0065] A method for preparing a germanate red light perovskite quantum dot glass with high luminous efficiency, comprising the following steps:
[0066] (1) H3BO3, GeO2, ZnO, CaO, Cs2CO3, PbO, NaI, NbBr and Nb2O5 are mixed and melted in a muffle furnace to obtain a glass melt; the molar ratio of H3BO3, GeO2, ZnO, CaO, Cs2CO3, PbO, NaI, NbBr and Nb2O5 is 40:40:4:3:4.5:2.5:2:4:2.8; the melting holding temperature is 1000°C, and the melting holding time is 20 minutes;
[0067] (2) pouring the glass melt obtained in step (1) onto a preheating plate, and then transferring it to an annealing furnace for annealing to obtain a glass block; the annealing temperature is 350° C., and the annealing time is 3 hours;
[0068] (3) The glass block obtained in step (2) is heat-treated to obtain a high-luminescence-efficiency germanate red-light perovskite quantum dot glass, which is denoted as PG4; the heat treatment is carried out at a holding temperature of 520° C. for a holding time of 4 h.
[0069] Example 5
[0070] A method for preparing a germanate red light perovskite quantum dot glass with high luminous efficiency, comprising the following steps:
[0071] (1) H3BO3, GeO2, ZnO, CaO, Cs2CO3, PbO, NaI, NbBr and Nb2O5 are mixed and melted in a muffle furnace to obtain a glass melt; the molar ratio of H3BO3, GeO2, ZnO, CaO, Cs2CO3, PbO, NaI, NbBr and Nb2O5 is 40:40:4:3:4.5:2.5:2:4:3.5; the melting holding temperature is 1000°C, and the melting holding time is 20 minutes;
[0072] (2) pouring the glass melt obtained in step (1) onto a preheating plate, and then transferring it to an annealing furnace for annealing to obtain a glass block; the annealing temperature is 350° C., and the annealing time is 3 hours;
[0073] (3) The glass block obtained in step (2) is heat-treated to obtain a high-luminescence-efficiency germanate red-light perovskite quantum dot glass, which is denoted as PG5; the heat treatment is carried out at a holding temperature of 520° C. for a holding time of 4 h.
[0074] Comparative Example 1
[0075] A method for preparing germanate red light perovskite quantum dot glass, comprising the following steps:
[0076] (1) H3BO3, GeO2, ZnO, CaO, Cs2CO3, PbO, NaI and NbBr are mixed and melted in a muffle furnace to obtain a glass melt; the molar ratio of H3BO3, GeO2, ZnO, CaO, Cs2CO3, PbO, NaI and NbBr is 40:40:4:3:4.5:2.5:2:4; the melting holding temperature is 1000° C., and the melting holding time is 20 min;
[0077] (2) pouring the glass melt obtained in step (1) onto a preheating plate, and then transferring it to an annealing furnace for annealing to obtain a glass block; the annealing temperature is 350° C., and the annealing time is 3 hours;
[0078] (3) The glass block obtained in step (2) is subjected to heat treatment to obtain germanate red light perovskite quantum dot glass, which is denoted as PG0; the heat treatment is carried out at a holding temperature of 520° C. and a heat treatment time of 4 h.
[0079] The germanate red light perovskite quantum dot glasses obtained in Examples 1 to 5 and Comparative Example 1 were characterized by X-ray diffraction (XRD) (D2 phase shifter, Bruker, Karlsruhe). The results are shown in FIG. Figure 1As shown. Figure 1 It can be seen that the XRD diffraction peaks corresponding to the CsPbBrI2 perovskite quantum dots were observed in the XRD diffraction pattern, proving that the CsPbBrI2 perovskite quantum dots were precipitated in the glass.
[0080] The germanate red light perovskite quantum dot glass obtained in Example 3 was observed using a JEOL JEM-F200 transmission electron microscope (TEM). The TEM image obtained is as follows: Figure 2 The size distribution histogram obtained is shown in Figure 3 The obtained HTEM image is shown in Figure 4 As shown. Figures 2 to 4 It can be seen that many black spherical particles are precipitated in the glass. The average particle size of the particles is about 5.89 nanometers, and the interplanar spacing is 0.216 nanometers, corresponding to the (220) crystal plane of CsPbBrI2 perovskite quantum dots, further proving that CsPbBrI2 perovskite quantum dots have been successfully precipitated in germanate glass.
[0081] The germanate red light perovskite quantum dot glass obtained in Examples 1 to 5 and Comparative Example 1 was observed using a fluorescence spectrometer with a 450W xenon lamp. The emission spectra obtained are as follows: Figure 5 As shown. Figure 5 It can be seen that the emission spectrum peak of the germanate red light perovskite quantum dot glass is located at 660-680 nanometers.
[0082] The germanate red light perovskite quantum dot glass obtained in Example 3 was observed using an FTIR infrared spectrometer. The obtained FTIR graph is as follows: Figure 6 The Raman spectrum obtained is shown in Figure 7 As shown. Figure 6 and Figure 7 It can be seen that with the increase of Nb 5+ With the addition of ions, the bridging oxygen bonds of the [BO4] tetrahedron are destroyed, and the number of [BO3] triangles increases, causing the glass network structure to become loose, providing space for the growth and nucleation of perovskite quantum dots.
[0083] Figure 8 This is the heating spectrum of the germanate red light perovskite quantum dot glass obtained in Example 3. Fig. 9 This is the cooling spectrum of the germanate red light perovskite quantum dot glass obtained in Example 3. Fig.10 This is the luminescence intensity variation curve of the germanate red light perovskite quantum dot glass obtained in Example 3 during the heating and cooling process. Figures 8 to 10It can be seen that when the temperature gradually rises from room temperature, the luminescence intensity of CsPbBrI2 perovskite quantum dot glass gradually decreases, and when the temperature gradually drops to room temperature, the luminescence of perovskite quantum dot glass gradually recovers, and at the same temperature, the intensity is even higher than when heated, indicating that CsPbBrI2 perovskite quantum dot glass has excellent temperature resilience.
[0084] From the above analysis, it can be seen that at the optimal in situ crystallization temperature, red light CsPbBrI2 perovskite quantum dot glass with high luminescence efficiency is prepared in germanate glass, and the prepared CsPbBrI2 perovskite quantum dot glass has excellent temperature resilience.
[0085] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing a high luminous efficiency germanate red light perovskite quantum dot glass, comprising the following steps: (1) H3BO3, GeO2, ZnO, CaO, Cs2CO3, PbO, NaI, NbBr and Nb2O5 are mixed and melted to obtain a glass melt; (2) annealing the glass melt obtained in step (1) to obtain a glass block; (3) heat-treating the glass block obtained in step (2) to obtain a germanate red light perovskite quantum dot glass with high luminous efficiency.
2. The preparation method according to claim 1, characterized in that: In the step (1), the molar ratio of H3BO3, GeO2, ZnO, CaO, Cs2CO3, PbO, NaI, NbBr and Nb2O5 is (35-55): (25-40): (4-6): (3-5): (4-6): (2.5-3): 2: 4: (0.7-3.5).
3. The preparation method according to claim 2, characterized in that: The molar ratio of H3BO3, GeO2, ZnO, CaO, Cs2CO3, PbO, NaI, NbBr and Nb2O5 is 40:40:4:3:4.5:2.5:2:4:(0.7~3.5).
4. The preparation method according to claim 1, characterized in that: The melting and holding temperature in the step (1) is 900-1050° C., and the melting and holding time is 10-40 minutes.
5. The preparation method according to claim 4, characterized in that: The melting and holding temperature is 1000° C., and the melting and holding time is 20 minutes.
6. The preparation method according to claim 1, characterized in that: The holding temperature of the annealing treatment in the step (2) is 300-400° C., and the holding time of the annealing treatment is 2-5 hours.
7. The preparation method according to claim 6, characterized in that: The holding temperature of the annealing treatment is 350° C., and the holding time of the annealing treatment is 3 hours.
8. The preparation method according to claim 1, characterized in that: The heat treatment in step (3) is carried out at a holding temperature of 500 to 550° C. and for a holding time of 3 to 6 hours.
9. The preparation method according to claim 8, characterized in that: The heat treatment is carried out at a holding temperature of 520° C. and for a holding time of 4 hours.
10. The high luminous efficiency germanate red light perovskite quantum dot glass prepared by the preparation method according to any one of claims 1 to 9.
Citation Information
Patent Citations
Sm3+: CsPbBr3 quantum dot microcrystalline glass material
CN109626827A
Al < 3 + >-doped CsPbBr3 quantum dot glass ceramic and preparation method thereof
CN114634312A
Full-inorganic perovskite quantum dot microcrystalline glass material and preparation method thereof
CN115124247A
Inorganic perovskite quantum dot glass and preparation method thereof
CN115849721A
Rare earth ion doped phosphate perovskite quantum dot glass and preparation method thereof
CN118344003A