Perovskite quantum dot glass with adjustable luminescence color and preparation method thereof

By introducing Eu3+ and Tm3+ ions on the surface of phosphate glass and using mechanical crystallization method, the problem of stability and multi-color coexistence of perovskite quantum dot material is solved, and three colors of red-green-blue are realized on the same piece of glass The adjustable luminescence simplifies the preparation process and reduces energy consumption.

CN118908569AInactive Publication Date: 2024-11-08CHINA JILIANG UNIV
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410973103.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Traditional perovskite quantum dot materials have shortcomings in stability and multi-color coexistence, and cannot achieve adjustable luminescence in three colors: red-green-blue on the same piece of glass.

Method used

By mixing NH4H2PO4, Pb3O4, SiO2, Cs2CO3, PbBr2, NaBr, Eu2O3 and Tm2O3 with melting, annealing and mechanical grinding, Eu3+ and Tm3+ ions were introduced, and CsPbBr3 quantum dots were obtained on the surface of phosphate glass by mechanical crystallization, achieving red-green -The three colors of blue glow.

Benefits of technology

It realizes the coexistence of multiple colors and adjustable colors on the same piece of glass, and the preparation process is simple, no high-temperature heat treatment is required, and it has energy-saving effects, which is suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118908569A_ABST
    Figure CN118908569A_ABST
Patent Text Reader

Abstract

The invention provides luminescent color adjustable perovskite quantum dot glass and a preparation method thereof, and belongs to the field of solid luminescent materials. Eu < 3 + > and Tm < 3 + > are introduced into perovskite quantum dot glass, due to the fact that different rare earth ions have different energy level structures, the glass can have different light emitting colors, mechanical grinding operation is introduced, CsPbBr3 quantum dots are obtained on the surface of the Eu < 3 + > / Tm < 3 + > co-doped phosphate glass through a mechanical crystallization method, and the CsPbBr3 quantum dots can be obtained. Therefore, red-green-blue light can be emitted on the same glass, and the problem that rare earth ions are in the glass and cannot emit light of different colors after Eu < 3 + > and Tm < 3 + > are introduced in a conventional scheme can be solved; meanwhile, the preparation method is simple, high-temperature heat treatment is not needed in the preparation process, the good energy-saving effect is achieved, and large-scale production can be achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of solid luminescent materials, and in particular to a perovskite quantum dot glass with adjustable luminescent color and a preparation method thereof. Background Art

[0002] In recent years, perovskite quantum dot materials have been widely used in solar cells, LEDs, liquid crystal displays and other fields due to their high fluorescence quantum yield, narrow emission band, and continuously adjustable luminescence in the entire visible light band. However, due to their low formation energy and ionic crystal properties, the colloidal quantum dots obtained by traditional hot injection methods have poor stability. Ligand modification, core-shell structure and organic encapsulation can improve the stability of perovskite quantum dots to a certain extent, but since these encapsulation methods cannot well separate the perovskite quantum dots from the surrounding environment, the improvement of the stability of perovskite quantum dots is still not ideal. Glass, as an ancient optical material, has a dense structure and good physical and chemical stability. Thanks to the dense structure and high transparency of glass materials, encapsulating perovskite quantum dots in a glass matrix can not only significantly improve the stability of perovskite quantum dots, but also maintain its good luminescence properties.

[0003] Although perovskite quantum dot glass can achieve adjustable luminescence in the entire visible light band, only one color can be presented on the same piece of glass, and the coexistence of the three colors of red, green and blue (at least two colors) cannot be achieved, resulting in the application of perovskite quantum dot glass still being greatly limited.

[0004] Therefore, how to make perovskite quantum dot glass achieve the coexistence of multiple colors and adjustable colors has become a technical problem that needs to be solved urgently in this field. Summary of the invention

[0005] The purpose of the present invention is to provide a perovskite quantum dot glass with adjustable luminescent color and a preparation method thereof. The CsPbBr3 quantum dot glass prepared by the preparation method provided by the present invention can realize red, green and blue three-color luminescence on the same piece of glass, and the color is adjustable.

[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0007] The present invention provides a method for preparing perovskite quantum dot glass with adjustable luminescent color, comprising the following steps:

[0008] (1) NH4H2PO4, Pb3O4, SiO2, Cs2CO3, PbBr2, NaBr, Eu2O3 and Tm2O3 are mixed and melted to obtain a glass melt;

[0009] (2) annealing the glass melt obtained in step (1) to obtain a glass block;

[0010] (3) Mechanically grinding the glass block obtained in step (2) to obtain perovskite quantum dot glass with adjustable luminescent color.

[0011] Preferably, the molar ratio of NH4H2PO4, Pb3O4, SiO2, Cs2CO3, PbBr2, NaBr, Eu2O3 and Tm2O3 in step (1) is (65-75):(5-15):(1-5):(5-10):(5-10):(5-10):(0.3-0.6):(0.3-0.6).

[0012] Preferably, the molar ratio of NH4H2PO4, Pb3O4, SiO2, Cs2CO3, PbBr2, NaBr, Eu2O3 and Tm2O3 is 65:7:3:10:10:5:(0.3~0.6):(0.3~0.6).

[0013] Preferably, the melting and holding temperature in step (1) is 700-750° C., and the melting and holding time is 10-40 min.

[0014] Preferably, the melting holding temperature is 720° C., and the melting holding time is 20 min.

[0015] Preferably, the holding temperature of the annealing treatment in step (2) is 150-200° C., and the holding time of the annealing treatment is 2-5 hours.

[0016] Preferably, the holding temperature of the annealing treatment is 180° C., and the holding time of the annealing treatment is 3 hours.

[0017] Preferably, the mechanical grinding time in step (3) is 1 to 10 minutes.

[0018] Preferably, the mechanical grinding time in step (3) is 3 to 7 minutes.

[0019] The present invention provides perovskite quantum dot glass with adjustable luminescent color prepared by the preparation method described in the above technical solution.

[0020] The present invention provides a method for preparing perovskite quantum dot glass with adjustable luminescent color, comprising the following steps: (1) mixing NH4H2PO4, Pb3O4, SiO2, Cs2CO3, PbBr2, NaBr, Eu2O3 and Tm2O3 and melting them to obtain a glass melt; (2) annealing the glass melt obtained in step (1) to obtain a glass block; (3) mechanically grinding the glass block obtained in step (2) to obtain perovskite quantum dot glass with adjustable luminescent color. The present invention introduces Eu into the perovskite quantum dot glass. 3+ and Tm 3+ , and introduced mechanical grinding operation, through mechanical crystallization method in Eu 3+ / Tm 3+ CsPbBr3 quantum dots are obtained on the surface of co-doped phosphate glass, so that red, green and blue three-color luminescence can be achieved on the same piece of glass, which can solve the problem that different rare earth ions have different energy level structures, so that the glass can have different luminescent colors; at the same time, the preparation method provided by the present invention is simple, and no high-temperature heat treatment is required during the preparation process, which has good energy-saving effect and can be mass-produced. The results of the embodiment show that the CsPbBr3 quantum dot glass provided by the present invention can achieve red, green and blue three-color luminescence on the same piece of glass, and the luminescence effect will be adjusted accordingly with the change of grinding time. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 Characteristic absorption, emission and excitation spectra of the GPG sample obtained in Comparative Example 1;

[0022] Figure 2 TEM image of the GPG sample obtained in Comparative Example 1;

[0023] Figure 3 is the size distribution histogram of the GPG sample obtained in Comparative Example 1;

[0024] Figure 4 This is the HTEM image of the GPG sample obtained in Comparative Example 1;

[0025] Figure 5 This is the emission spectrum of the GPG-Eu0.6 sample obtained in Comparative Example 2;

[0026] Figure 6 This is the emission spectrum of the GPG-Tm0.6 sample obtained in Comparative Example 3;

[0027] Figure 7 The emission spectra of the GPG-Eu0.3Tm0.3 samples obtained in Examples 1 to 4 and Comparative Example 4;

[0028] Figure 8The color coordinates of the GPG-Eu0.3Tm0.3 samples obtained in Examples 1 to 4 and Comparative Example 4 on the CIE chromaticity diagram. DETAILED DESCRIPTION

[0029] The present invention provides a method for preparing perovskite quantum dot glass with adjustable luminescent color, comprising the following steps:

[0030] (1) NH4H2PO4, Pb3O4, SiO2, Cs2CO3, PbBr2, NaBr, Eu2O3 and Tm2O3 are mixed and melted to obtain a glass melt;

[0031] (2) annealing the glass melt obtained in step (1) to obtain a glass block;

[0032] (3) Mechanically grinding the glass block obtained in step (2) to obtain perovskite quantum dot glass with adjustable luminescent color.

[0033] The present application mixes NH4H2PO4, Pb3O4, SiO2, Cs2CO3, PbBr2, NaBr, Eu2O3 and Tm2O3 and melts them to obtain a glass melt.

[0034] In the present invention, unless otherwise specified, the raw materials used are commercially available products well known to those skilled in the art or products prepared using known techniques.

[0035] In the present invention, the molar ratio of NH4H2PO4, Pb3O4, SiO2, Cs2CO3, PbBr2, NaBr, Eu2O3 and Tm2O3 is preferably (65-75): (5-15): (1-5): (5-10): (5-10): (5-10): (0.3-0.6): (0.3-0.6), and more preferably 65: 7: 3: 10: 10: 5: (0.3-0.6): (0.3-0.6). The present invention can control the amount of Eu in the glass by controlling the relationship between the amounts of the raw materials. 3+ and Tm 3+ The doping amount can further adjust the luminescence effect of the glass.

[0036] The present invention has no particular limitation on the specific operation of the mixing, which can be determined according to the technical common sense of those skilled in the art.

[0037] In the present invention, the melting is preferably carried out in a muffle furnace. The present invention has no particular limitation on the specific model of the muffle furnace, and a commercially available muffle furnace well known to those skilled in the art can be used.

[0038] In the present invention, the melting holding temperature is preferably 700-750°C, more preferably 720°C; the melting holding time is preferably 10-40 minutes, more preferably 20 minutes. The present invention can ensure that the raw materials are completely melted to form a uniform glass melt by controlling the melting process parameters.

[0039] After obtaining the glass melt, the present invention performs annealing treatment on the glass melt to obtain a glass block.

[0040] In the present invention, the annealing treatment method is preferably to pour the glass melt into a mold and quickly transfer it to an annealing furnace for annealing treatment; the material of the mold is preferably brass or stainless steel. The present invention can avoid excessive internal stress caused by rapid cooling of the glass melt in the air, which causes the glass block to crack.

[0041] In the present invention, the holding temperature of the annealing treatment is preferably 150-200°C, more preferably 180°C; the holding time of the annealing treatment is preferably 2-5h, more preferably 3h. The present invention can eliminate the internal stress in the glass block through annealing treatment, laying a foundation for subsequent mechanical grinding; by controlling the process parameters of the annealing treatment, it can be ensured that the internal stress is eliminated as much as possible.

[0042] After obtaining the glass block, the present invention mechanically grinds the glass block to obtain perovskite quantum dot glass with adjustable luminescent color.

[0043] In the present invention, the mechanical grinding method is preferably: placing the glass block on sandpaper for manual mechanical grinding. The present invention has no special requirements on the specific source and mesh number of the sandpaper, and commercially available sandpaper well known to those skilled in the art can be used.

[0044] In the present invention, the mechanical grinding time is preferably 1 to 10 minutes, more preferably 1 minute, 2 minutes, 3 minutes, 4 minutes, 5 minutes, 6 minutes, 7 minutes, 8 minutes, 9 minutes or 10 minutes. The present invention adopts the method of mechanical grinding, through the action of mechanical force, so that CsPbBr3 quantum dots can be on Eu 3+ / Tm 3+ The co-doped phosphate glass surface is precipitated, so that Eu can be simultaneously realized on a piece of glass 3+ 、Tm 3+ Red, blue and green light emission of CsPbBr3 quantum dots; by controlling the time of mechanical grinding, tunability of different colors can be achieved.

[0045] The present invention introduces Eu into perovskite quantum dot glass 3+ and Tm 3+ , and introduced mechanical grinding operation, through mechanical crystallization method in Eu3+ / Tm 3+ CsPbBr3 quantum dots are obtained on the surface of co-doped phosphate glass, so that red, green and blue light emission can be achieved on the same piece of glass, which can solve the problem that different rare earth ions have different energy level structures, so that the glass can have different light emission colors; at the same time, the preparation method provided by the present invention is simple, no high-temperature heat treatment is required during the preparation process, it has good energy-saving effect, and can be mass-produced.

[0046] The present invention provides perovskite quantum dot glass with adjustable luminescent color prepared by the preparation method described in the above technical solution.

[0047] The perovskite quantum dot glass with adjustable luminescent color provided by the present invention can realize red, green and blue luminescence on the same piece of glass.

[0048] The technical solutions in the present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0049] Example 1

[0050] A method for preparing perovskite quantum dot glass with adjustable luminescent color, comprising the following steps:

[0051] (1) NH4H2PO4, Pb3O4, SiO2, Cs2CO3, PbBr2, NaBr, Eu2O3 and Tm2O3 are mixed and melted in a muffle furnace to obtain a glass melt; the molar ratio of NH4H2PO4, Pb3O4, SiO2, Cs2CO3, PbBr2, NaBr, Eu2O3 and Tm2O3 is 65:7:3:10:10:5:0.3:0.3; the melting holding temperature is 720°C, and the melting holding time is 20 minutes;

[0052] (2) pouring the glass melt obtained in step (1) into a brass mold, and quickly transferring it to an annealing furnace for annealing to obtain a glass block; the annealing temperature is 180° C., and the annealing time is 3 hours;

[0053] (3) The glass block obtained in step (2) is placed on sandpaper for manual mechanical grinding to obtain a perovskite quantum dot glass with adjustable luminescent color, which is recorded as GPG-Eu0.3Tm0.3; the mechanical grinding time is 1 min.

[0054] Example 2

[0055] A method for preparing perovskite quantum dot glass with adjustable luminescent color, comprising the following steps:

[0056] (1) NH4H2PO4, Pb3O4, SiO2, Cs2CO3, PbBr2, NaBr, Eu2O3 and Tm2O3 are mixed and melted in a muffle furnace to obtain a glass melt; the molar ratio of NH4H2PO4, Pb3O4, SiO2, Cs2CO3, PbBr2, NaBr, Eu2O3 and Tm2O3 is 65:7:3:10:10:5:0.3:0.3; the melting holding temperature is 720°C, and the melting holding time is 20 minutes;

[0057] (2) pouring the glass melt obtained in step (1) into a brass mold, and quickly transferring it to an annealing furnace for annealing to obtain a glass block; the annealing temperature is 180° C., and the annealing time is 3 hours;

[0058] (3) The glass block obtained in step (2) is placed on sandpaper for manual mechanical grinding to obtain a perovskite quantum dot glass with adjustable luminescent color, which is recorded as GPG-Eu0.3Tm0.3; the mechanical grinding time is 3 minutes.

[0059] Example 3

[0060] A method for preparing perovskite quantum dot glass with adjustable luminescent color, comprising the following steps:

[0061] (1) NH4H2PO4, Pb3O4, SiO2, Cs2CO3, PbBr2, NaBr, Eu2O3 and Tm2O3 are mixed and melted in a muffle furnace to obtain a glass melt; the molar ratio of NH4H2PO4, Pb3O4, SiO2, Cs2CO3, PbBr2, NaBr, Eu2O3 and Tm2O3 is 65:7:3:10:10:5:0.3:0.3; the melting holding temperature is 720°C, and the melting holding time is 20 minutes;

[0062] (2) pouring the glass melt obtained in step (1) into a brass mold, and quickly transferring it to an annealing furnace for annealing to obtain a glass block; the annealing temperature is 180° C., and the annealing time is 3 hours;

[0063] (3) The glass block obtained in step (2) is placed on sandpaper for manual mechanical grinding to obtain a perovskite quantum dot glass with adjustable luminescent color, which is recorded as GPG-Eu0.3Tm0.3; the mechanical grinding time is 5 minutes.

[0064] Example 4

[0065] A method for preparing perovskite quantum dot glass with adjustable luminescent color, comprising the following steps:

[0066] (1) NH4H2PO4, Pb3O4, SiO2, Cs2CO3, PbBr2, NaBr, Eu2O3 and Tm2O3 are mixed and melted in a muffle furnace to obtain a glass melt; the molar ratio of NH4H2PO4, Pb3O4, SiO2, Cs2CO3, PbBr2, NaBr, Eu2O3 and Tm2O3 is 65:7:3:10:10:5:0.3:0.3; the melting holding temperature is 720°C, and the melting holding time is 20 minutes;

[0067] (2) pouring the glass melt obtained in step (1) into a brass mold, and quickly transferring it to an annealing furnace for annealing to obtain a glass block; the annealing temperature is 180° C., and the annealing time is 3 hours;

[0068] (3) The glass block obtained in step (2) is placed on sandpaper for manual mechanical grinding to obtain a perovskite quantum dot glass with adjustable luminescent color, which is recorded as GPG-Eu0.3Tm0.3; the mechanical grinding time is 10 minutes.

[0069] Comparative Example 1

[0070] A method for preparing green light emitting CsPbBr3 quantum dot glass, comprising the following steps:

[0071] (1) NH4H2PO4, Pb3O4, SiO2, Cs2CO3, PbBr2 and NaBr are mixed and melted in a muffle furnace to obtain a glass melt; the molar ratio of NH4H2PO4, Pb3O4, SiO2, Cs2CO3, PbBr2 and NaBr is 65:7:3:10:10:5; the melting holding temperature is 720° C., and the melting holding time is 20 min;

[0072] (2) pouring the glass melt obtained in step (1) into a brass mold, and quickly transferring it to an annealing furnace for annealing to obtain a glass block; the annealing temperature is 180° C., and the annealing time is 3 hours;

[0073] (3) The glass block obtained in step (2) is placed on sandpaper for manual mechanical grinding to obtain green light emitting CsPbBr3 quantum dot glass, denoted as GPG; the mechanical grinding time is 3 minutes.

[0074] Comparative Example 2

[0075] A red-green light tunable emission Eu 3+ The preparation method of CsPbBr3 doped quantum dot glass consists of the following steps:

[0076] (1) NH4H2PO4, Pb3O4, SiO2, Cs2CO3, PbBr2, NaBr and Eu2O3 are mixed and melted in a muffle furnace to obtain a glass melt; the molar ratio of NH4H2PO4, Pb3O4, SiO2, Cs2CO3, PbBr2, NaBr and Eu2O3 is 65:7:3:10:10:5:0.3; the melting holding temperature is 720°C and the melting holding time is 20 minutes;

[0077] (2) pouring the glass melt obtained in step (1) into a brass mold, and quickly transferring it to an annealing furnace for annealing to obtain a glass block; the annealing temperature is 180° C., and the annealing time is 3 hours;

[0078] (3) The glass block obtained in step (2) is placed on sandpaper for manual mechanical grinding to obtain red-green light tunable emission Eu 3+ The CsPbBr3 quantum dot glass is doped and is denoted as GPG-Eu0.3. The mechanical grinding time is 3 minutes.

[0079] Comparative Example 3

[0080] A blue-green light tunable emission Tm 3+ The preparation method of CsPbBr3 doped quantum dot glass consists of the following steps:

[0081] (1) NH4H2PO4, Pb3O4, SiO2, Cs2CO3, PbBr2, NaBr and Tm2O3 are mixed and melted in a muffle furnace to obtain a glass melt; the molar ratio of NH4H2PO4, Pb3O4, SiO2, Cs2CO3, PbBr2, NaBr and Tm2O3 is 65:7:3:10:10:5:0.3; the melting holding temperature is 720°C, and the melting holding time is 20 minutes;

[0082] (2) pouring the glass melt obtained in step (1) into a brass mold, and quickly transferring it to an annealing furnace for annealing to obtain a glass block; the annealing temperature is 180° C., and the annealing time is 3 hours;

[0083] (3) The glass block obtained in step (2) is placed on sandpaper for manual mechanical grinding to obtain a blue-green light tunable emission Tm 3+The CsPbBr3 quantum dot glass is doped and is denoted as GPG-Tm0.3; the mechanical grinding time is 3 minutes.

[0084] Comparative Example 4

[0085] A CsPbBr3 quantum dot glass, wherein the mechanical grinding time in the preparation method is 0 min, and other conditions are the same as those in Example 1, and is recorded as GPG-Eu0.3Tm0.3.

[0086] The GPG sample obtained in Comparative Example 1 was tested using a PerkinElmer Lambda absorption spectrometer to obtain a broadband absorption spectrum in the range of 200 to 800 nm. The GPG sample obtained in Comparative Example 1 was tested using a fluorescence spectrometer with a 450W xenon lamp to obtain a broadband excitation and emission spectrum with a Gaussian symmetric spectrum. The results are shown in FIG. Figure 1 As shown. Figure 1 It can be seen that the characteristic broadband excitation spectrum, broadband absorption spectrum and typical Gass symmetric emission spectrum in the figure indicate that the detected green light emission does come from CsPbBr3 quantum dots, indicating that CsPbBr3 quantum dots can be obtained on the glass surface through mechanical crystallization.

[0087] The GPG sample obtained in Comparative Example 1 was observed using a JEOL JEM-F200 transmission electron microscope (TEM). The TEM image obtained is as follows: Figure 2 The size distribution histogram obtained is shown in Figure 3 The obtained HTEM image is shown in Figure 4 As shown. Figures 2 to 4 It can be seen that many spherical particles are precipitated on the glass surface, and uniformly distributed black spherical particles are obtained. The average particle size of the particles is about 9.68nm, and the interplanar spacing is 0.148nm, which corresponds to the (200) crystal plane of CsPbBr3 quantum dots. This further proves that CsPbBr3 quantum dots have been successfully prepared on the phosphate glass surface by mechanical crystallization method.

[0088] The GPG-Eu0.6 sample obtained in Comparative Example 2 was observed using a fluorescence spectrometer with a 450W xenon lamp. The emission spectrum of the obtained GPG-Eu0.6 sample is as follows: Figure 5 As shown. Figure 5 It can be seen that when the excitation wavelength is 365nm, the GPG-Eu0.6 sample has both green light emission from CsPbBr3 quantum dots and Eu 3+ The characteristic red light emission of ions, the emission peak corresponding to CsPbBr3 quantum dots at around 518nm and the emission peak corresponding to Eu 3+ The characteristic emission peak of the ion indicates that 3+Ion doping and mechanical crystallization methods can achieve red-green tunable emission on phosphate glass.

[0089] The GPG-Tm0.6 sample obtained in Comparative Example 3 was observed using a fluorescence spectrometer with a 450W xenon lamp. The emission spectrum of the obtained GPG-Tm0.6 sample is as follows: Figure 6 As shown. Figure 6 It can be seen that when the excitation wavelength is 365nm, the GPG-Tm0.6 sample has both green light emission of CsPbBr3 quantum dots and Tm 3+ The characteristic blue light emission of ions indicates that the 3+ Ion doping and mechanical crystallization methods can achieve blue-green tunable emission on phosphate glass.

[0090] The GPG-Eu0.3Tm0.3 samples obtained in Examples 1 to 4 and Comparative Example 4 were observed using a fluorescence spectrometer with a 450W xenon lamp. The results are as follows: Figure 7 As shown, the color coordinates of the corresponding samples on the CIE chromaticity diagram are as follows Figure 8 As shown. Figure 7 and Figure 8 It can be seen that when the grinding time increases from 0 to 10 min, the green light emission peak corresponding to the CsPbBr3 quantum dots gradually increases. When the grinding time increases to 10 min, the sample almost only has green light emission from CsPbBr3 quantum dots, and the corresponding color coordinates gradually transition from blue-violet light to cold white light and cyan light to green light.

[0091] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing perovskite quantum dot glass with adjustable luminescent color, comprising the following steps: (1) NH4H2PO4, Pb3O4, SiO2, Cs2CO3, PbBr2, NaBr, Eu2O3 and Tm2O3 are mixed and melted to obtain a glass melt; (2) annealing the glass melt obtained in step (1) to obtain a glass block; (3) Mechanically grinding the glass block obtained in step (2) to obtain perovskite quantum dot glass with adjustable luminescent color.

2. The preparation method according to claim 1, characterized in that: In the step (1), the molar ratio of NH4H2PO4, Pb3O4, SiO2, Cs2CO3, PbBr2, NaBr, Eu2O3 and Tm2O3 is (65-75): (5-15): (1-5): (5-10): (5-10): (5-10): (0.3-0.6): (0.3-0.6).

3. The preparation method according to claim 2, characterized in that: The molar ratio of NH4H2PO4, Pb3O4, SiO2, Cs2CO3, PbBr2, NaBr, Eu2O3 and Tm2O3 is 65:7:3:10:10:5:(0.3~0.6):(0.3~0.6).

4. The preparation method according to claim 1, characterized in that: The melting and holding temperature in the step (1) is 700-750° C., and the melting and holding time is 10-40 minutes.

5. The preparation method according to claim 4, characterized in that: The melting holding temperature is 720° C., and the melting holding time is 20 minutes.

6. The preparation method according to claim 1, characterized in that: The holding temperature of the annealing treatment in the step (2) is 150-200° C., and the holding time of the annealing treatment is 2-5 hours.

7. The preparation method according to claim 6, characterized in that: The holding temperature of the annealing treatment is 180° C., and the holding time of the annealing treatment is 3 hours.

8. The preparation method according to claim 1, characterized in that: The mechanical grinding time in step (3) is 1 to 10 minutes.

9. The preparation method according to claim 8, characterized in that: The mechanical grinding time is 3 to 7 minutes.

10. Perovskite quantum dot glass with adjustable luminescent color prepared by the preparation method according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Rare earth doped luminescent glass, and preparation method thereof

    CN103936281A

  • Borosilicate rare earth luminescent microcrystalline glass, and preparation method and application thereof

    CN110467351A

  • Wavelength-adjustable color-changing luminescent material and preparation method thereof

    CN116285982A

  • Illuminant with variable emission and method for controlled changing of the color impression of a light source

    DE102015101413A1