Method for strengthening high-aluminum microcrystalline glass, high-aluminum microcrystalline glass and application of high-aluminum microcrystalline glass
By regulating the Zn2+ content and optimizing the composition of high-aluminum glass, high-aluminum microcrystalline glass with excellent mechanical properties and light transmittance is formed, which solves the problem of increasing viscosity and crystallization loss caused by excessive Al2O3 in high-aluminum glass, and realizes industrialization Feasibility and application value of production.
Patent Information
- Application Number
- CN202411156652.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-22
- Publication Date
- 2024-11-08
AI Technical Summary
The excessive Al2O3 content in high alumina glass leads to an increase in the viscosity of the glass liquid, the crystallization component range is narrow, and the crystals are prone to be out of control and excessive growth, affecting the light transmittance and mechanical properties of the glass.
By regulating the content of Zn2+, it can not only molten high-aluminum glass but also participate in the formation of ZnAl2O4 crystals, optimize the network structure of the glass, and improve crystallization ability and mechanical properties. The specific steps include mixing the glass raw materials, melting, forming, annealing, nucleating and crystallizing, ensuring that the ZnO content is 8 to 22 wt%, and the Al2O3 content is above 25 wt%, forming a high-aluminum micrometer with excellent mechanical properties and light transmittance. Crystal glass.
The mechanical properties and light transmittance optimization of high-aluminum microcrystalline glass have been achieved. The Vickers hardness is greater than 10GPa, the light transmittance is greater than 80%. The preparation method is simple and low cost, and it is suitable for communications, biology, building materials and other fields.
Smart Images

Figure CN118908577A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of microcrystalline glass, and in particular to a method for strengthening high-aluminum microcrystalline glass, high-aluminum microcrystalline glass and applications thereof. Background Art
[0002] As an ancient and traditional material, glass is widely used in industries such as communications, biology, building materials, information display, optoelectronics and the automotive industry. In order to meet the higher requirements of the rapidly developing era for glass, aluminosilicate glass has become a hot topic of research. The main components of aluminosilicate glass are SiO2 and Al2O3, both of which can be used as network formers. In the glass network, they exist in the form of [TO4] (T=Si, Al) tetrahedrons. Due to its high strength and excellent light transmittance, chemical stability and thermal stability, it is widely used in consumer electronics, aerospace and optical imaging.
[0003] However, the strength and impact resistance of ordinary aluminosilicate glass cannot meet the needs of cutting-edge fields. The emergence of high-aluminum glass solves these problems. Its high aluminum content improves the integrity of the glass network and increases the intrinsic strength of the glass. In order to further improve the mechanical and optical properties of high-aluminum glass, a crystal nucleating agent is added to the glass component and heat treated to obtain high-aluminum microcrystalline glass. High-aluminum microcrystalline glass takes into account the characteristics of both glass and ceramics, has adjustable mechanical properties, optical properties and chemical stability, and has become an excellent candidate material for application in cutting-edge fields.
[0004] ZnAl2O4 is a kind of spinel mineral. It is an oxide mineral of zinc and aluminum with a very high Mohs hardness (7.5-8.0). For fully dense ZnAl2O4 ceramics, the Young's modulus can reach about 240GPa. If ZnAl2O4 nanocrystals are precipitated in glass, the hardness and fracture toughness of microcrystalline glass can be effectively improved. Therefore, the precipitation of ZnAl2O4 nanocrystals in high-aluminum glass can obtain microcrystalline glass with extremely high hardness and modulus, making the application range of high-aluminum glass more extensive.
[0005] However, there are still some problems to be solved in high-aluminum glass. For example, too high Al2O3 content in the glass will increase the viscosity of the glass liquid, resulting in a narrow range of crystallization components, and the crystals are prone to uncontrolled excessive growth, causing the glass to become devitrified. Summary of the invention
[0006] In view of this, the object of the present invention is to provide a method for strengthening high-aluminum microcrystalline glass, high-aluminum microcrystalline glass and its application. 2+ The content of ZnAl2O4 can be regulated to help melt high-aluminum glass and participate in the formation of ZnAl2O4 crystals. In addition, the regulation method provided by the present invention is simple and efficient, has low cost, is easy to industrially scale up, and has great application value.
[0007] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0008] The present invention provides a method for strengthening high-aluminum glass-ceramics, comprising the following steps:
[0009] The glass raw materials are mixed according to the composition of high-aluminum glass-ceramics to obtain a mixture; the content of ZnO in the high-aluminum glass-ceramics is 8 to 22 wt %;
[0010] Melting the mixture to obtain molten glass;
[0011] The glass liquid is sequentially molded and annealed to obtain basic glass;
[0012] The base glass is sequentially nucleated and crystallized to obtain high-aluminum glass-ceramics.
[0013] Preferably, the content of Al2O3 in the high-aluminum glass-ceramics is above 25wt%.
[0014] Preferably, the composition of the high-aluminum glass-ceramics includes: 34.5wt% to 45.5wt% SiO2; 25wt% to 35wt% Al2O3; 8wt% to 22wt% ZnO; 1wt% to 7wt% MgO; 1wt% to 7wt% Na2O; 1wt% to 7wt% Li2O; 4wt% to 8wt% TiO2; and 1wt% to 2wt% ZrO2.
[0015] Preferably, the mixing is grinding mixing.
[0016] Preferably, the melting temperature is 1600-1700° C.; and the melting time is 3-5 hours.
[0017] Preferably, the molding is performed in a graphite mold; the graphite mold is preheated before use; the preheating temperature is 600-700°C.
[0018] Preferably, the annealing temperature is 600-650° C.; and the annealing time is 2-4 hours.
[0019] Preferably, the nucleation temperature is the glass transition temperature of the base glass, and the holding time is 3 to 6 hours.
[0020] Preferably, the crystallization temperature is 800-1000° C., and the holding time is 1-3 hours.
[0021] The present invention provides high-aluminum glass-ceramics prepared by the method described in the above technical solution.
[0022] The present invention provides the application of the high-aluminum glass-ceramics described in the above technical solution in the fields of communication, biology, building materials, information display, optoelectronics or automobile industry.
[0023] The present invention provides a method for strengthening high-aluminum glass-ceramics, comprising the following steps: mixing glass raw materials according to the composition of high-aluminum glass-ceramics to obtain a mixture; the content of ZnO in the high-aluminum glass-ceramics is 8-22wt%; melting the mixture to obtain glass liquid; molding and annealing the glass liquid in sequence to obtain a basic glass; and nucleating and crystallizing the basic glass in sequence to obtain a high-aluminum glass-ceramics. In the present invention, Zn 2+ It acts as both a network modifier and a network former in glass components. A small amount of Zn in high-aluminum glass 2+ In order to balance the charge of [AlO4], it will preferentially exist in the glass network gap as a network modifier. 2+ When introduced, it will be a four-coordinated network former. 2+ When introduced, it will depolymerize part of the network structure as a network modifier, thereby improving the crystallization ability of the glass. 2+ When the ZnAl2O4 is precipitated, the precipitation of ZnAl2O4 is promoted, and the precipitation of ZnAl2O4 improves the mechanical properties while ensuring the light transmittance. 2+ To prepare high-aluminum glass-ceramics with strong crystallization ability, stable structure and excellent mechanical properties.
[0024] The high-aluminum glass-ceramics strengthened after adjusting the components of the present invention not only has excellent mechanical strength but also has good light transmittance. Experimental results show that the Vickers hardness of the high-aluminum glass-ceramics obtained by the present invention is greater than 10GPa and the light transmittance is greater than 80%.
[0025] The preparation method of the high-aluminum glass-ceramics of the present invention is simple, easy to operate, low in cost, easy to mass-produce, and has excellent mechanical properties, chemical stability and transmittance after component regulation. It has important application value in industries such as communications, biology, building materials, information display, optoelectronics and automobile industry. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 The SEM images of the high-aluminum glass-ceramics in Examples 1 to 4;
[0027] Figure 2 TEM images of the high-aluminum glass-ceramics in Example 4, wherein (a) is a TEM image and (b) is a selected area electron diffraction image;
[0028] Figure 3 XRD patterns of high-aluminum glass-ceramics in Examples 1 to 4;
[0029] Figure 4 is the Raman spectrum of the high-aluminum glass-ceramics in Examples 1 to 4;
[0030] Figure 5 The XPS spectra of the high-aluminum glass-ceramics in Examples 1 to 4;
[0031] Figure 6 FT-IR spectra of high-aluminum glass-ceramics in Examples 1 to 4;
[0032] Figure 7 These are performance test diagrams of high-aluminum glass-ceramics in Examples 1 to 4, wherein (a) is a Vickers hardness test diagram, and (b) is a light transmittance test diagram;
[0033] Figure 8 This is the SEM image of the high-aluminum glass-ceramics in Example 8. DETAILED DESCRIPTION
[0034] The present invention provides a method for strengthening high-aluminum glass-ceramics, comprising the following steps:
[0035] The glass raw materials are mixed according to the composition of high-aluminum glass-ceramics to obtain a mixture; the content of ZnO in the high-aluminum glass-ceramics is 8 to 22 wt %;
[0036] Melting the mixture to obtain molten glass;
[0037] The glass liquid is sequentially molded and annealed to obtain basic glass;
[0038] The base glass is sequentially nucleated and crystallized to obtain high-aluminum glass-ceramics.
[0039] The present invention mixes glass raw materials according to the composition of high-aluminum glass-ceramics to obtain a mixture. In the present invention, the content of ZnO in the high-aluminum glass-ceramics is 8-22wt%, and is preferably 8wt%, 10wt%, 12wt%, 14wt%, 16wt%, 18wt%, 20wt% or 22wt%. The present invention increases the content of ZnO to reduce all other components except ZrO2 and TiO2. The present invention only needs to adjust the content of ZnO. 2+ The content of can obtain high aluminum microcrystalline glass with higher mechanical and optical properties.
[0040] In the present invention, the content of Al2O3 in the high-aluminum glass-ceramics is preferably above 25wt%. In the present invention, the high aluminum content improves the intrinsic strength of the glass and refines the grains. 2+ The content improves the crystallization ability of the glass, improving the mechanical properties while ensuring the light transmittance.
[0041] In the present invention, the composition of the high-aluminum glass-ceramics is preferably oxide. In the present invention, the composition of the high-aluminum glass-ceramics preferably includes: 34.5wt% to 45.5wt% SiO2; 25wt% to 35wt% Al2O3; 8wt% to 22wt% ZnO; 1wt% to 7wt% MgO; 1wt% to 7wt% Na2O; 1wt% to 7wt% Li2O; 4wt% to 8wt% TiO2; 1wt% to 2wt% ZrO2. In the present invention, the composition of the high-aluminum microcrystalline glass more preferably includes: 34wt% to 40wt% SiO2; 28wt% to 30wt% Al2O3; 10wt% to 20wt% ZnO; 3wt% to 5wt% MgO; 3wt% to 5wt% Na2O; 3wt% to 5wt% Li2O; 4wt% to 7wt% TiO2; and 1wt% to 2wt% ZrO2.
[0042] In the present invention, SiO2 can form a network structure using the structural elements of silicon-oxygen tetrahedrons, forming the basic structure of silicates; high Al2O3 content can form a glass network and refine the grains, thereby improving the intrinsic strength of the glass; precise control of Zn 2+ The increase of the content not only improves the refractory problem of high-aluminum glass, but also promotes the precipitation of nano-crystalline ZnAl2O4.
[0043] In the present invention, the glass raw materials include oxides and carbonates, and specifically preferably include Li2CO3, Na2CO3, MgO, ZnO, Al2O3, SiO2, ZrO2 and TiO2. The entire preparation process of the present invention only requires oxides and carbonates as raw materials, and the Li content in the high-aluminum glass raw materials is low, which reduces the cost and makes it easy to mass-produce industrial products.
[0044] In the present invention, the mixing is preferably grinding mixing. In the present invention, the grinding time is preferably 1 to 4 hours, more preferably 2 hours. In the present invention, the particle size of the mixed material is preferably 2 to 20 μm, more preferably 2 to 15 μm.
[0045] After obtaining the mixture, the present invention melts the mixture to obtain glass liquid. In the present invention, the melting temperature is preferably 1600-1700°C, more preferably 1650°C; the melting time is preferably 3-5h, more preferably 3-4h. In the present invention, the melting is preferably carried out in a quartz crucible. In a specific embodiment of the present invention, the glass liquid is clarified.
[0046] After obtaining the glass liquid, the present invention sequentially shapes and anneals the glass liquid to obtain the basic glass. In the present invention, the shaping is preferably performed in a graphite mold; the graphite mold is preferably preheated before use; the preheating temperature is preferably 600-700°C, more preferably 625-650°C.
[0047] In the present invention, the annealing temperature is preferably lower than the glass transition temperature of the base glass. In the present invention, the annealing temperature is preferably 600-650°C, more preferably 625°C; the annealing time is preferably 2-4 hours. In the present invention, the annealing is preferably performed in a muffle furnace. The present invention eliminates thermal stress and prevents cracking by annealing.
[0048] After obtaining the base glass, the present invention sequentially performs nucleation and crystallization on the base glass to obtain high-aluminum glass-ceramics. In the present invention, the nucleation and crystallization are preferably performed in a muffle furnace.
[0049] In the present invention, the nucleation temperature is preferably the glass transition temperature of the base glass, specifically preferably 650-750°C; the holding time is preferably 3-6h, more preferably 3-5h. In the present invention, the heating rate from room temperature to the nucleation temperature is preferably 1-15°C / min, more preferably 3-12°C / min.
[0050] In the present invention, the crystallization temperature is preferably 800-1000°C, more preferably 810-990°C; the holding time is preferably 1-3h, more preferably 2-2.5h. In the present invention, the heating rate from the nucleation temperature to the crystallization temperature is preferably 1-10°C / min, more preferably 5°C / min.
[0051] The present invention provides high-aluminum glass-ceramics prepared by the method described in the above technical solution.
[0052] In the present invention, the grain size of the crystallites in the high-aluminum glass-ceramics is preferably 3 to 30 nm.
[0053] The present invention provides the application of the high-aluminum glass-ceramics described in the above technical solution in the fields of communication, biology, building materials, information display, optoelectronics or automobile industry.
[0054] The technical solutions in the present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0055] Example 1
[0056] Glass raw materials are weighed in the proportion of 4wt% Li2O, 1wt% Na2O, 7wt% MgO, 8wt% ZnO, 30wt% Al2O3, 40wt% SiO2, 2wt% ZrO2 and 8wt% TiO2, wherein Li2O and Na2O are introduced through their carbonates (Li2CO3 and Na2CO3). The weighed glass raw materials are ground for 2h to mix evenly and sieved to obtain a mixture with a particle size of 2μm;
[0057] The mixed material is placed in a quartz crucible, the quartz crucible is placed in a high-temperature electric furnace, and melted at 1700° C. for 3 hours to obtain glass liquid;
[0058] The glass liquid is poured into a graphite mold preheated at 600° C. to form the glass, the graphite mold is placed in a muffle furnace, annealed at 600° C. for 2 hours, and cooled to room temperature to obtain a basic glass; a glass transition temperature of the basic glass is 696° C. and a crystallization temperature is 1000° C. obtained by simultaneous thermal analysis (DSC);
[0059] The base glass is placed in a muffle furnace, heated to a glass transition temperature of 696°C at a rate of 3°C / min, and nucleated for 3 hours; then rapidly heated to a crystallization temperature of 1000°C of the base glass at a rate of 5°C / min, and crystallized for 1 hour to obtain high-aluminum microcrystalline glass with a grain size of 3nm.
[0060] Example 2
[0061] The glass raw materials are weighed in the proportion of 2wt% Li2O, 3wt% Na2O, 2wt% MgO, 12wt% ZnO, 34wt% Al2O3, 41wt% SiO2, 2wt% ZrO2 and 4wt% TiO2, wherein Li2O and Na2O are introduced through their carbonates. The weighed glass raw materials are ground for 2h to mix evenly and sieved to obtain a mixture with a particle size of 4μm;
[0062] The mixed material is placed in a quartz crucible, the quartz crucible is placed in a high-temperature electric furnace, and melted at 1650° C. for 5 hours to obtain glass liquid;
[0063] The glass liquid is poured into a graphite mold preheated at 625° C. to form the glass, the graphite mold is placed in a muffle furnace, annealed at 625° C. for 4 hours, and cooled to room temperature to obtain a basic glass; the glass transition temperature of the basic glass is obtained by simultaneous thermal analysis (DSC) to be 687° C., and the crystallization temperature is 850° C.;
[0064] The base glass is placed in a muffle furnace, heated to a glass transition temperature of 687°C at a rate of 5°C / min, and nucleated for 6 hours; then rapidly heated to a crystallization temperature of 850°C for the base glass at a rate of 5°C / min, and crystallized for 2 hours to obtain high-aluminum microcrystalline glass with a grain size of 10 nm.
[0065] Example 3
[0066] The glass raw materials are weighed in the proportion of 3.5wt% Li2O, 2.5wt% Na2O, 3.5wt% MgO, 16wt% ZnO, 34wt% Al2O3, 35wt% SiO2, 1.5wt% ZrO2 and 4wt% TiO2, wherein Li2O and Na2O are introduced through their carbonates. The weighed glass raw materials are ground for 2h to mix evenly and sieved to obtain a mixture with a particle size of 5μm;
[0067] The mixed material is placed in a quartz crucible, the quartz crucible is placed in a high-temperature electric furnace, and melted at 1600° C. for 4 hours to obtain glass liquid;
[0068] The glass liquid is poured into a graphite mold preheated at 600° C. to form the glass, the graphite mold is placed in a muffle furnace, annealed at 600° C. for 2 hours, and cooled to room temperature to obtain a basic glass; a glass transition temperature of the basic glass is 681° C. and a crystallization temperature is 810° C. obtained by using simultaneous thermal analysis (DSC);
[0069] The base glass is placed in a muffle furnace, heated to a glass transition temperature of 681°C at a rate of 12°C / min for nucleation for 4.5 hours; then rapidly heated to a crystallization temperature of 810°C for the base glass at a rate of 5°C / min for crystallization for 2 hours to obtain high-aluminum microcrystalline glass with a grain size of 18nm.
[0070] Example 4
[0071] The glass raw materials are weighed in the proportion of 7wt% Li2O, 7wt% Na2O, 1wt% MgO, 20wt% ZnO, 25wt% Al2O3, 35wt% SiO2, 1wt% ZrO2 and 4wt% TiO2, wherein Li2O and Na2O are introduced through their carbonates. The weighed glass raw materials are ground for 2h to mix evenly and sieved to obtain a mixture with a particle size of 8μm;
[0072] The mixed material is placed in a quartz crucible, the quartz crucible is placed in a high-temperature electric furnace, and melted at 1650° C. for 3 hours to obtain glass liquid;
[0073] The glass liquid is poured into a graphite mold preheated at 600° C. to form the glass, the graphite mold is placed in a muffle furnace, annealed at 600° C. for 2 hours, and cooled to room temperature to obtain a basic glass; a glass transition temperature of the basic glass is 679° C. and a crystallization temperature is 800° C. obtained by simultaneous thermal analysis (DSC);
[0074] The base glass is placed in a muffle furnace, heated to a glass transition temperature of 679°C at a rate of 15°C / min for nucleation for 6 hours; then rapidly heated to a crystallization temperature of 800°C for the base glass at a rate of 5°C / min for crystallization for 3 hours to obtain high-aluminum microcrystalline glass with a grain size of 26nm.
[0075] Example 5
[0076] The glass raw materials are weighed in the proportion of 1.5wt% Li2O, 1wt% Na2O, 1wt% MgO, 10wt% ZnO, 35wt% Al2O3, 45.5wt% SiO2, 2wt% ZrO2 and 4wt% TiO2, wherein Li2O and Na2O are introduced through their carbonates. The weighed glass raw materials are ground for 2h to mix evenly and sieved to obtain a mixture with a particle size of 11μm;
[0077] The mixed material is placed in a quartz crucible, the quartz crucible is placed in a high-temperature electric furnace, and melted at 1600° C. for 5 hours to obtain glass liquid;
[0078] The glass liquid is poured into a graphite mold preheated at 625° C. to form the glass, the graphite mold is placed in a muffle furnace, annealed at 625° C. for 2 hours, and cooled to room temperature to obtain a basic glass; the glass transition temperature of the basic glass is 689° C. and the crystallization temperature is 900° C. obtained by simultaneous thermal analysis (DSC);
[0079] The base glass is placed in a muffle furnace, heated to a glass transition temperature of 689°C at a rate of 9°C / min for nucleation for 3 hours; then rapidly heated to a crystallization temperature of 900°C for the base glass at a rate of 5°C / min for crystallization for 1 hour to obtain high-aluminum glass-ceramics with a grain size of 7nm.
[0080] Example 6
[0081] Glass raw materials are weighed in the proportion of 5wt% Li2O, 2wt% Na2O, 2wt% MgO, 14wt% ZnO, 30wt% Al2O3, 41wt% SiO2, 2wt% ZrO2 and 4wt% TiO2, wherein Li2O and Na2O are introduced through their carbonates. The weighed glass raw materials are ground for 2h to mix evenly and sieved to obtain a mixture with a particle size of 15μm;
[0082] The mixed material is placed in a quartz crucible, the quartz crucible is placed in a high-temperature electric furnace, and melted at 1700° C. for 1 hour to obtain glass liquid;
[0083] The glass liquid is poured into a graphite mold preheated at 600° C. to form the glass, the graphite mold is placed in a muffle furnace, annealed at 650° C. for 4 hours, and cooled to room temperature to obtain a basic glass; the glass transition temperature of the basic glass is 680° C. and the crystallization temperature is 990° C. obtained by using simultaneous thermal analysis (DSC);
[0084] The base glass is placed in a muffle furnace, heated to a glass transition temperature of 680°C at a rate of 1°C / min for nucleation for 3 hours; then rapidly heated to a crystallization temperature of 990°C for the base glass at a rate of 5°C / min for crystallization for 2 hours to obtain high-aluminum glass-ceramics with a grain size of 14 nm.
[0085] Example 7
[0086] The glass raw materials are weighed in the proportion of 3wt% Li2O, 1wt% Na2O, 1wt% MgO, 18wt% ZnO, 30wt% Al2O3, 39wt% SiO2, 1wt% ZrO2 and 7wt% TiO2, wherein Li2O and Na2O are introduced through their carbonates. The weighed glass raw materials are ground for 2h to mix evenly and sieved to obtain a mixture with a particle size of 17μm;
[0087] The mixed material is placed in a quartz crucible, the quartz crucible is placed in a high-temperature electric furnace, and melted at 1650° C. for 3.5 hours to obtain glass liquid;
[0088] The glass liquid is poured into a graphite mold preheated at 600° C. to form the glass, the graphite mold is placed in a muffle furnace, annealed at 600° C. for 3 hours, and cooled to room temperature to obtain a basic glass; a glass transition temperature of the basic glass is 681° C. and a crystallization temperature is 800° C. obtained by simultaneous thermal analysis (DSC);
[0089] The base glass is placed in a muffle furnace, heated to a glass transition temperature of 681°C at a rate of 10°C / min for nucleation for 3 hours; then rapidly heated to a crystallization temperature of 800°C for the base glass at a rate of 5°C / min for crystallization for 2 hours to obtain high-aluminum microcrystalline glass with a grain size of 22nm.
[0090] Example 8
[0091] The glass raw materials are weighed in the proportion of 1wt% Li2O, 3.5wt% Na2O, 6wt% MgO, 22wt% ZnO, 25wt% Al2O3, 34.5wt% SiO2, 2wt% ZrO2 and 6wt% TiO2, wherein Li2O and Na2O are introduced through their carbonates. The weighed glass raw materials are ground for 2h to mix evenly and sieved to obtain a mixture with a particle size of 20μm;
[0092] The mixed material is placed in a quartz crucible, the quartz crucible is placed in a high-temperature electric furnace, and melted at 1650° C. for 3 hours to obtain glass liquid;
[0093] The glass liquid is poured into a graphite mold preheated at 650° C. to form the glass, the graphite mold is placed in a muffle furnace, annealed at 650° C. for 2 hours, and cooled to room temperature to obtain a basic glass; the glass transition temperature of the basic glass is obtained by simultaneous thermal analysis (DSC) to be 675° C., and the crystallization temperature is 840° C.;
[0094] The base glass is placed in a muffle furnace, heated to a glass transition temperature of 675°C at a rate of 5°C / min for nucleation for 6 hours; then rapidly heated to a crystallization temperature of 840°C for the base glass at a rate of 5°C / min for crystallization for 1 hour to obtain high-aluminum glass-ceramics with a grain size of 30nm.
[0095] Test Case
[0096] Figure 1 is the SEM image of the high-aluminum glass-ceramics in Examples 1 to 4. Figure 1 It can be seen that the crystals are small in size and evenly distributed.
[0097] Figure 2 is the TEM image of the high-aluminum glass-ceramics in Example 4, Figure 2 (a) is a TEM image, (b) is a selected area electron diffraction image, Figure 2 It can be seen that the crystals are closely arranged and the crystal phase is consistent with the XRD results.
[0098] Figure 3 is the XRD pattern of the high aluminum glass-ceramics in Examples 1 to 4, Figure 3 It can be seen that the crystal peak of ZnAl2O4 gradually increases.
[0099] Figure 4 is the Raman spectrum of the high-aluminum glass-ceramics in Examples 1 to 4, Figure 4 It can be seen that the characteristic peak of ZnAl2O4 gradually increases, and the characteristic peak of the glass phase gradually weakens as the crystallization process proceeds and then slightly increases.
[0100] Figure 5 is the XPS spectrum of the high-aluminum glass-ceramics in Examples 1 to 4, Figure 5 It can be seen that the Zn ratio in the crystal phase increases continuously and then tends to be stable.
[0101] Figure 6 is the FT-IR spectrum of the high-aluminum glass-ceramics in Examples 1 to 4, Figure 6 It can be seen that the broad peak of the glass phase in the high wavenumber region shows a splitting trend, indicating that the increase in Zn content has a dual effect of depolymerization and stabilization on the residual glass phase.
[0102] Figure 7 The performance test diagram of high aluminum glass-ceramics in Examples 1 to 4 is shown in FIG. Figure 7 (a) is a Vickers hardness test chart, the hardness can reach up to 10.03GPa; (b) is a transmittance test chart, the transmittance is up to 80%. Figure 7 It can be seen that the appropriate Zn content can take into account both mechanical properties and transmittance.
[0103] Figure 8 is the SEM image of the high-aluminum glass-ceramics in Example 8. Figure 8 It can be seen that excess Zn 2+ The introduction of leads to the precipitation of large-sized crystals.
[0104] It can be seen from the above examples that the high-aluminum glass-ceramics strengthened by adjusting the components of the present invention not only has excellent mechanical strength but also has good light transmittance. In addition, the method of strengthening the glass-ceramics of the present invention is simple and low-cost, and is not only easy to convert into an industrial production process line but also easy to large-scale industrial production.
[0105] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for strengthening high-aluminum glass-ceramics, The following steps are involved: The glass raw materials are mixed according to the composition of high-aluminum glass-ceramics to obtain a mixture; the content of ZnO in the high-aluminum glass-ceramics is 8 to 22 wt %; Melting the mixture to obtain molten glass; The glass liquid is sequentially molded and annealed to obtain basic glass; The base glass is sequentially nucleated and crystallized to obtain high-aluminum glass-ceramics.
2. The method according to claim 1, It is characterized in that The Al in the high-aluminum glass-ceramics 2 O 3 The content is above 25wt%.
3. The method according to claim 1 or 2, It is characterized in that The composition of the high-aluminum glass-ceramics includes: 34.5wt% to 45.5wt% of SiO 2 ; 25wt%~35wt%Al 2 O 3 ; 8wt% to 22wt% ZnO; 1wt% to 7wt% MgO; 1wt% to 7wt% Na 2 O; 1 wt% to 7 wt% Li 2 O; 4wt% to 8wt% TiO 2 ; 1wt%~2wt% ZrO 2 .
4. The method according to claim 1, It is characterized in that The mixing is grinding mixing.
5. The method according to claim 1, It is characterized in that The melting temperature is 1600-1700° C.; the melting time is 3-5 hours.
6. The method according to claim 1, It is characterized in that The molding is carried out in a graphite mold; the graphite mold is preheated before use; the preheating temperature is 600-700°C.
7. The method according to claim 1, It is characterized in that The annealing temperature is 600-650° C.; the annealing time is 2-4 hours.
8. The method according to claim 1, It is characterized in that The nucleation temperature is the glass transition temperature of the base glass, and the heat preservation time is 3 to 6 hours.
9. The method according to claim 1, It is characterized in that The crystallization temperature is 800-1000° C., and the insulation time is 1-3 hours.
10. High-aluminum glass-ceramics prepared by the method described in any one of claims 1 to 9.
11. Application of the high-aluminum glass-ceramics according to claim 10 in the fields of communications, biology, building materials, information display, optoelectronics or automobile industry.
Citation Information
Patent Citations
Colorless transparent magnesium-aluminum-silicon microcrystalline glass and preparation method thereof
CN115057621A
Glass ceramic, glass ceramic product and manufacturing method thereof
CN116621455A
Transparent microcrystalline glass with high scratch resistance
CN118164677A