Glass powder and preparation method thereof, atomizing core and preparation method thereof
By using glass powder composed of silicon oxide, main softener and secondary softener, the sintering temperature and shrinkage of the atomized core are reduced, and the use effect of thick film printing technology on large-capacity atomizer is solved. The best problem is to achieve high strength and low cost porous ceramic atomized core preparation.
Patent Information
- Application Number
- CN202410955695.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-16
- Publication Date
- 2024-11-08
AI Technical Summary
In the prior art, the atomized core prepared by thick film printing technology has poor use effect on large-capacity atomizers. The steel sheet heating sheet is prone to oxidation under high temperature sintering, resulting in an increase in resistance and shrinkage of the atomized core matrix. The high rate leads to poor coordination between the heating plate and the substrate and increases cost.
Glass powder including silicon oxide, main softener (boron oxide, zinc oxide, bismuth oxide) and secondary softener (potassium oxide, lithium oxide) is used to prepare low-temperature porous ceramic atomization by reducing the softening point and expansion coefficient and increasing the strength. Core, reduces the sintering temperature and shrinkage rate, and improves structural strength.
It effectively reduces the sintering temperature and shrinkage rate of the atomized core, improves structural strength, reduces energy consumption and cost, ensures good cooperation between the heating plate and the substrate, and improves the service life and yield rate of the product.
Smart Images

Figure CN118908578A_ABST
Abstract
Description
Technical Field
[0001] The present application belongs to the field of atomization technology, and specifically relates to glass powder and a preparation method thereof, an atomization core and a preparation method thereof. Background Art
[0002] Large-capacity atomizers are quite popular in the market, but the atomizer cores prepared by thick film printing technology do not work well on large-capacity atomizers. Therefore, the steel sheet type heating sheet inlay technology is usually used to prepare porous ceramic atomizer cores to meet the use requirements. However, the steel sheet is prone to oxidation under high-temperature sintering, resulting in an increase in the resistance of the heating sheet, and the steel sheet material basically does not shrink, but the atomizer core matrix will shrink significantly during the sintering process, resulting in the atomizer core matrix and the heating sheet not being able to fit well together. Summary of the invention
[0003] In view of this, the first aspect of the present application provides a glass powder, which includes silicon oxide, a main softener, and a secondary softener, the main softener includes at least one of boron oxide, zinc oxide, and bismuth oxide, and the secondary softener includes at least one of potassium oxide and lithium oxide.
[0004] The glass powder provided in the first aspect of the present application is one of the important raw materials for preparing the atomizer core matrix. The glass powder provided in the present application mainly includes silicon oxide, a main softener, and a secondary softener. Silicon oxide is the main component in the glass powder, which is equivalent to the matrix skeleton. The main softener and the secondary softener can also be understood as the first softener and the second softener, which are mainly used to reduce the softening point of the glass powder, so that the glass powder has a low softening point and reduce the softening temperature of the glass powder. Among them, the main softener plays a major role in reducing the softening temperature, and the secondary softener plays a secondary and auxiliary role in reducing the softening temperature. And through the mutual cooperation of silicon oxide, the main softener, and the secondary softener, the expansion coefficient of the glass powder can also be reduced, and the strength of the glass powder can be improved.
[0005] In summary, the glass powder provided in the present application has the characteristics of low softening point, low expansion coefficient and high strength. When the atomizer core is subsequently prepared, the sintering temperature and shrinkage rate of the atomizer core can be reduced, and the strength of the atomizer core can be improved.
[0006] Wherein, by mass percentage, the silicon oxide is 5%-10%, the boron oxide is 35%-50%, the zinc oxide is 10%-20%, the bismuth oxide is 20%-40%, the potassium oxide is 0%-5%, and the lithium oxide is 0%-5%.
[0007] A second aspect of the present application provides a method for preparing glass powder, the preparation method comprising:
[0008] Providing silicon oxide, a main softener, and a secondary softener, wherein the main softener includes at least one of boron oxide, zinc oxide, and bismuth oxide, and the secondary softener includes at least one of potassium oxide and lithium oxide;
[0009] The silicon oxide, the main softener, and the secondary softener are uniformly mixed and dried to obtain a mixture;
[0010] Melting the mixed material to obtain a molten liquid, and quenching the molten liquid to obtain a glass material;
[0011] The glass material is crushed, ball-milled, dried and sieved in sequence to obtain glass powder.
[0012] The second aspect of the present application provides a method for preparing glass powder, which adopts silicon oxide, a main softener, and a secondary softener, so that the prepared glass powder has the characteristics of low softening point, low expansion coefficient, and high strength. When the atomizer core is subsequently prepared, the sintering temperature and shrinkage rate of the atomizer core can be reduced, and the strength of the atomizer core can be improved.
[0013] The third aspect of the present application provides a method for preparing an atomizer core, the preparation method comprising:
[0014] Providing a solute and a solvent, wherein the solute includes a matrix material, a pore former, and the glass powder provided in the first aspect of the present application;
[0015] The solute is dried, and the dried solute and the solvent are treated with wax to obtain a mixed slurry;
[0016] Providing a heating sheet, processing the mixed slurry and the heating sheet through a slip injection molding process, so that the mixed slurry forms an atomizer core matrix embryo, and fixing the heating sheet to the atomizer core matrix embryo, to obtain an atomizer core embryo;
[0017] The atomizer core embryo is processed through a degreasing process and a sintering process to obtain an atomizer core.
[0018] The preparation method of the atomizer core provided in the third aspect of the present application can reduce the sintering temperature during the sintering process, reduce the shrinkage rate of the atomizer core, and improve the structural strength of the atomizer core by adopting the glass powder provided in the first aspect of the present application.
[0019] Wherein, in the sintering process, the maximum sintering temperature is no more than 600°C.
[0020] Wherein, the matrix material includes silicon oxide, aluminum oxide, and diatomaceous earth.
[0021] Wherein, the particle size of the silicon oxide is 18-24 μm, the particle size of the aluminum oxide is 30-35 μm, and the particle size of the diatomaceous earth is 2-6 μm.
[0022] Wherein, the particle size of the pore-forming agent is 50-70 μm.
[0023] Wherein, by mass percentage, the silicon oxide is 15%-25%, the aluminum oxide is 20%-30%, the diatomaceous earth is 2%-8%, the pore-forming agent is 10%-25%, and the glass powder is 20%-30%.
[0024] The fourth aspect of the present application provides an atomizer core, which is prepared by the preparation method of the atomizer core provided by the third aspect of the present application.
[0025] The atomizer core provided in the fourth aspect of the present application is prepared by adopting the preparation method of the atomizer core provided in the third aspect of the present application, which can reduce the sintering temperature during the sintering process, reduce the shrinkage rate of the atomizer core, and improve the structural strength of the atomizer core. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] In order to more clearly illustrate the technical solutions in the implementation modes of the present application, the drawings required for use in the implementation modes of the present application will be described below.
[0027] Figure 1 This is a process flow chart of a method for preparing glass powder in one embodiment of the present application.
[0028] Figure 2 This is a process flow chart of a method for preparing an atomizer core in one embodiment of the present application.
[0029] Figure 3 A schematic diagram of the three-dimensional structure of the atomizer core provided in one embodiment of the present application
[0030] Description of labels:
[0031] Atomizer core - 1, atomizer core base - 10, heating sheet - 20. DETAILED DESCRIPTION
[0032] The following are preferred implementations of the present application. It should be noted that, for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present application, and these improvements and modifications are also considered to be within the scope of protection of the present application.
[0033] Before introducing the technical solution of the present application, the technical problems in the related technology are introduced in detail.
[0034] Large-capacity atomizers are quite popular in the market. The preparation process of the heating sheet in the atomizer core is a thick film printing process. The thick film printing process can only be carried out on a plane, and there are many process flows, and the resistance value of the manufactured heating sheet varies greatly. Therefore, the atomizer core prepared by thick film printing technology is not effective in large-capacity atomizers. At present, steel sheet-type heating sheet inlay technology is usually used to prepare porous ceramic atomizer cores to meet the use requirements. Specifically, when the atomizer core matrix is made into a green body through molding processes such as injection molding and grouting molding, the prepared heating sheet is placed in the mold and directly fixed on the atomizer core matrix embryo, and then the atomizer core finished product is obtained through degreasing and high-temperature sintering.
[0035] However, the sintering temperature in the sintering process of the related technology is relatively high, for example, the sintering temperature is as high as 1000°C, which consumes a lot of energy. The steel sheet is easily oxidized at high temperature, which leads to an increase in the resistance of the heating sheet material, and the steel sheet material basically does not shrink, but the shrinkage rate of the atomizer core substrate is relatively large, for example, it can reach a shrinkage rate of 10%, the product size is not easy to control, and the yield rate is low, which increases the cost. This leads to poor bonding between the sintered finished heating sheet and the atomizer core substrate, and even causes the heating sheet to deform, and the atomizer core substrate and the heating sheet cannot fit together well. Therefore, the atomizer core is currently required to have the characteristics of a sufficiently low sintering temperature, small shrinkage, and high strength of use.
[0036] In view of this, in order to solve the above problems, the present application provides a glass powder. The glass powder provided in this embodiment includes silicon oxide, a main softener, and a secondary softener. The main softener includes at least one of boron oxide, zinc oxide, and bismuth oxide, and the secondary softener includes at least one of potassium oxide and lithium oxide.
[0037] Glass powder is one of the important raw materials for preparing the atomizer core, so the performance of the glass powder will affect the performance of the atomizer core. This embodiment solves the above technical problems by changing the performance of the glass powder, thereby changing the characteristics of the atomizer core and its preparation process. The glass powder in this embodiment mainly includes silicon oxide, a main softener, and a secondary softener. Silicon oxide is the main component in the glass powder, which is equivalent to the matrix skeleton. The main softener and the secondary softener can also be understood as the first softener and the second softener, which are mainly used to reduce the softening point of the glass powder, so that the glass powder has a low softening point, and reduce the softening temperature of the glass powder. The reduction in the softening temperature of the glass powder can reduce the sintering temperature during the subsequent sintering of the atomizer core, thereby avoiding oxidation of the heating plate. Among them, the main softener plays a major role in reducing the softening temperature, and the secondary softener plays a minor and auxiliary role in reducing the softening temperature. Therefore, the glass powder of this application can also be referred to as low-temperature glass powder.
[0038] The main softening agent includes at least one of boron oxide, zinc oxide, and bismuth oxide. This embodiment is schematically described by only using the main softening agent to include boron oxide, zinc oxide, and bismuth oxide at the same time. The secondary softening agent includes at least one of potassium oxide and lithium oxide. This embodiment is schematically described by only using the secondary softening agent to include potassium oxide and lithium oxide at the same time. The effect of boron oxide, zinc oxide, and bismuth oxide in reducing the softening temperature is greater than the effect of potassium oxide and lithium oxide in reducing the softening temperature.
[0039] In addition, the glass powder provided in this embodiment can not only reduce the softening temperature, but also reduce the expansion coefficient of the glass powder and improve the strength of the glass powder through the cooperation of silicon oxide, the main softener, and the secondary softener. The reduction in the expansion coefficient leads to a reduction in the shrinkage rate of the glass powder, thereby reducing the shrinkage rate of the atomizer core matrix during subsequent sintering overcharging, so as to better cooperate with the heating sheet. The improvement in the strength of the glass powder can also improve the overall structural strength of the atomizer core matrix.
[0040] In summary, this embodiment designs a glass powder system, adjusts the composition of the glass powder and the glass network structure, and prepares low-temperature glass powder with low softening point, low expansion coefficient and high hardness. When the atomizer core is subsequently prepared, the sintering temperature and shrinkage rate of the atomizer core can be reduced, and the strength of the atomizer core can be improved, thereby reducing energy consumption and reducing costs.
[0041] In this embodiment, by mass percentage, the silicon oxide is 5%-10%, the boron oxide is 35%-50%, the zinc oxide is 10%-20%, the bismuth oxide is 20%-40%, the potassium oxide is 0%-5%, and the lithium oxide is 0%-5%. By making the main softener include boron oxide, zinc oxide, and bismuth oxide at the same time, and the secondary softener include potassium oxide and lithium oxide at the same time, the glass powder composed of the above six components is used, and the above mixing ratio is used at the same time, the expansion coefficient can be better reduced on the basis of reducing the softening temperature, and the strength of the glass powder can be improved.
[0042] Please refer to Figure 1 , Figure 1 The process flow chart of the preparation method of glass powder in one embodiment of the present application is as follows. This embodiment provides a preparation method of glass powder, and the preparation method includes S100, S200, S300, and S400. S100, S200, S300, and S400 are described in detail as follows.
[0043] S100, providing silicon oxide, a main softener, and a secondary softener, wherein the main softener includes at least one of boron oxide, zinc oxide, and bismuth oxide, and the secondary softener includes at least one of potassium oxide and lithium oxide.
[0044] S200, the silicon oxide, the main softener, and the secondary softener are mixed evenly and dried to obtain a mixture.
[0045] S300, melting the mixed material to obtain a molten liquid, and quenching the molten liquid to obtain a glass material.
[0046] S400, crushing, ball-milling, drying and sieving the glass material in sequence to obtain glass powder.
[0047] In this embodiment, silicon oxide, a main softener, and a secondary softener can be used to prepare glass powder. The detailed introduction and beneficial effects of silicon oxide, the main softener, and the secondary softener have been described in detail above, and this embodiment will not be repeated here. In this embodiment, silicon oxide, the main softener, and the secondary softener can be weighed in a certain amount ratio. In this embodiment, boron oxide, silicon oxide, zinc oxide, bismuth oxide, potassium oxide, and lithium oxide can be weighed at the same time. Then put the above six raw materials into a mixing barrel for mixing for 1h-2h. Then put the evenly mixed powder into a drying box at 80°C to dry the moisture in the powder, and dry it for 30 minutes-60 minutes to obtain a dried mixture.
[0048] The mixture is then placed in a crucible and placed in a melting furnace for melting. The temperature can be gradually raised to 1200°C-1300°C and kept warm for 30 minutes. At this time, the solid powder will gradually turn into a molten liquid. The molten liquid is then poured into deionized water for quenching and cooling to room temperature to obtain a glass material. The strength of the glass material can be further improved by quenching and cooling.
[0049] After drying the glass material, the glass material is crushed to separate the glass material into fine particles, then ball-milled and dried, and finally sieved to obtain glass powder. Optionally, the sieve mesh number can be selected according to the actual demand for the size of the glass powder, for example, 300 mesh can be selected for sieving.
[0050] The method for preparing glass powder provided in this embodiment adopts silicon oxide, a main softener, and a secondary softener, so that the prepared glass powder has the characteristics of low softening point, low expansion coefficient, and high strength. When the atomizer core is subsequently prepared, the sintering temperature and shrinkage rate of the atomizer core can be reduced, and the strength of the atomizer core can be improved.
[0051] Please refer to Figure 2 , Figure 2 The process flow chart of the preparation method of the atomizer core in one embodiment of the present application is shown in FIG. This embodiment provides a preparation method of the atomizer core, and the preparation method includes S500, S600, S700, and S800. S500, S600, S700, and S800 are described in detail as follows.
[0052] S500, providing a solute and a solvent, wherein the solute includes a matrix material, a pore-forming agent, and the glass powder provided in the above-mentioned embodiment of the present application.
[0053] In order to prepare the atomizer core, the atomizer core matrix can be prepared first. The preparation of the atomizer core matrix is mainly composed of two types of raw materials: solute and solvent. The solute is mainly various solid powders. The solute includes a matrix material, a pore former, and a glass powder. The raw materials of various components can be weighed as needed, and the above raw materials can be evenly mixed together in a certain proportion, that is, mixed. Optionally, the solute solid powder can be weighed according to the mass ratio and placed on a three-dimensional mixer for mixing, for example, it can be mixed for 2h-3h. Among them, the matrix material is the main component of the atomizer core matrix, the glass powder is mainly used to bond various aggregates together in the subsequent sintering process to make it better shaped, and the pore former is mainly used to help the atomizer core matrix to form pores.
[0054] S600, drying the solute, and treating the dried solute with the solvent with wax to obtain a mixed slurry.
[0055] After the solutes are mixed, the solute solid powders can be placed in a drying oven for drying to remove the moisture adsorbed in the powders. Optionally, the solute solid powders can be placed in a drying oven at 100° C. and dried for 2-4 hours.
[0056] Then, the dried solute solid powder and the solvent are placed in a wax mixing machine for wax mixing, so that the solute solid powder is evenly dispersed in the solvent to obtain a mixed slurry for subsequent molding. Specifically, the solvent can be weighed in a certain proportion and placed in a wax mixing machine, set to a suitable temperature and speed, stirred for half an hour, and completely melted to a clear liquid state. Then, the solute solid powder is placed in a wax mixing machine for stirring, for example, stirring for 3h-5h, so that the solute and the molten solvent are evenly mixed to obtain a mixed slurry.
[0057] Optionally, the solvent includes but is not limited to at least one of paraffin, beeswax, polyethylene, and stearic acid.
[0058] Further optionally, calculated by mass percentage, paraffin is 12%-20%, beeswax is 1%-3%, polyethylene is 1%-3%, and stearic acid is 1%-3%.
[0059] Optionally, the mass of the solute is 72%-82% of the sum of the mass of the solute and the solvent. When the matrix material, the pore-forming agent, and the glass powder are weighed and mixed in a certain proportion, the solute has a mass W1. Similarly, after the solvent is weighed in a certain proportion, the solvent has a mass W2. When the wax is mixed with the solvent, the mass of the solute can be 72%-82% of the sum of the mass of the solute and the mass of the solvent, that is, W1 / (W1+W2) is 72%-82%. When it is less than 72% or greater than 82%, the atomizer core embryo will be difficult to form during hot pressing, which will reduce the various performances of the atomizer core.
[0060] Optionally, the temperature of the wax mixing machine is 90°C-100°C, and the rotation speed of the wax mixing machine is 40r / min-60r / min.
[0061] Optionally, the dried solid solute powder can be added to the wax mixing machine in multiple times to further improve the mixing effect of the solute and the solvent. Further optionally, the multiple times is 4-7 times.
[0062] S700, providing a heating sheet, processing the mixed slurry and the heating sheet through a slip injection molding process, so that the mixed slurry forms an atomizer core matrix embryo, and fixing the heating sheet to the atomizer core matrix embryo, to obtain an atomizer core embryo.
[0063] In this embodiment, a heating sheet is first prepared, that is, a steel sheet with a metal etching mesh is designed in advance, and then the mixed slurry and the heating sheet are processed through a grouting molding process, and the heating sheet is directly fixed on the atomizer core matrix embryo formed by the mixed slurry. At this time, the heating sheet and the atomizer core matrix embryo can be called an atomizer core embryo. Specifically, the mixed slurry can be placed in the barrel of the grouting machine, and the steel sheet heating sheet can be placed in the mold. After the grouting molding process, a regular-shaped atomizer core embryo with a heating sheet can be obtained. In addition, the use of a steel sheet heating sheet can be suitable for a large-capacity atomizer core and increase the service life of the atomizer core.
[0064] S800, the atomizer core embryo is processed through a degreasing process and a sintering process to obtain an atomizer core.
[0065] The atomizer core embryo can then be degreased and sintered. During the sintering process, the pore-forming agent and solvent in the atomizer core embryo will decompose and volatilize in various forms. Therefore, holes will be formed in the space originally occupied by the pore-forming agent and the solvent, thereby forming an atomizer core with a porous structure inside, which facilitates the circulation of the aerosol matrix inside the atomizer core, and finally prepares the atomizer core.
[0066] Specifically, the atomizer core embryo can be placed in a sintering furnace, heated to 90°C at 20-40°C / h, kept warm for 0.5-1h, heated to 160°C at 15-25°C / h, kept warm for 2-4h, heated to 280°C at 15-20°C / h, kept warm for 2-4h, heated to 340°C at 20-30°C / h, kept warm for 1-2h, heated to 420°C at 10-15°C / h, kept warm for 2-4h, heated to 500°C at 10-20°C / h, kept warm for 1-2h, heated to 500-600°C at 20-30°C / h, kept warm for 2-4h, and cooled to room temperature to obtain the prepared atomizer core.
[0067] In the related art, the sintering temperature is as high as 1000°C, which will cause the heating plate to oxidize. However, this embodiment uses the glass powder provided in the above embodiment of the present application, which can effectively reduce the sintering temperature of the atomizer core embryo. For example, in the sintering process, the maximum sintering temperature is not more than 600°C, thereby avoiding the oxidation of the heating plate. At the same time, since the expansion coefficient of the glass powder is relatively low, the shrinkage rate of the prepared atomizer core can also be reduced. In addition, since the strength of the glass powder is increased, the strength of the atomizer core can also be increased, thereby obtaining an atomizer core with low sintering temperature, small shrinkage rate, high strength, high porosity, and uniform pore size, good size control, high strength, and is conducive to automated production. Optionally, the maximum sintering temperature is 500°C-600°C.
[0068] In summary, the preparation method of the atomizer core provided in this embodiment reduces the sintering temperature, reduces energy consumption, and reduces costs by designing a glass powder system; through formula design, an atomizer core with a small shrinkage rate and stable size control is obtained, thereby improving the yield rate.
[0069] In this embodiment, the matrix material includes silicon oxide, aluminum oxide, and diatomaceous earth. Since the matrix material is a ceramic material, the atomizer core can also be called a ceramic atomizer core, and the atomizer core matrix can also be called a ceramic atomizer core matrix. By using the above three matrix materials and combining them with glass powder, the structural strength of the atomizer core matrix can be further improved.
[0070] It is worth noting that in this embodiment, the glass powder includes silicon oxide, and the matrix material also includes silicon oxide. However, during the sintering process, the solid silicon oxide of the glass powder will melt into irregular silicon oxide and bond the matrix material together. When cooled to room temperature, the silicon oxide of the glass powder will re-form into a solid. However, the silicon oxide of the matrix material always maintains a solid state. Therefore, even when performing subsequent electron microscopy analysis, the silicon oxide of the glass powder and the silicon oxide of the matrix material can be distinguished, that is, the silicon oxide with a regular spherical shape is the silicon oxide of the matrix material, and the irregular silicon oxide is the silicon oxide of the glass powder.
[0071] In this embodiment, the particle size of the silicon oxide is 18-24μm, the particle size of the aluminum oxide is 30-35μm, and the particle size of the diatomite is 2-6μm. On the basis of using silicon oxide, aluminum oxide, and diatomite, this embodiment also limits the particle size of the three materials. Specifically, the minimum particle size of diatomite is 2-6μm, the medium particle size of silicon oxide is 18-24μm, and the maximum particle size of aluminum oxide is 30-35μm. By using the mutual cooperation of three different particle sizes of small, medium and large, part of the medium particle size can be embedded in the gap of the large particle size, and the small particle size can be embedded in the gap between the medium particle size and the large particle size, so that the inside of the atomizer core matrix is more dense and the porosity is reduced. In this way, the shrinkage rate will be reduced accordingly due to the reduction of porosity during the sintering process, thereby further reducing the shrinkage rate of the atomizer core, for example, the shrinkage rate is 2%-3%, which is much less than 10% in the related art, with good size control, high strength, and conducive to automated production.
[0072] In this embodiment, the pore former is one of PS microspheres and PMMA, and the particle size of the pore former is 50-70 μm. By using the pore former of the above materials and controlling the particle size of the pore former to be 50-70 μm, that is, the particle size of the pore former is larger than the particle size of alumina with the largest particle size in the matrix material, that is, the particle size of the pore former is the largest, so when the pore former decomposes during the sintering process, the atomizer core matrix can have a higher porosity and pore size, and because the porosity at the matrix material is lower and the shrinkage rate is lower, the pore size of the finished atomizer core matrix is also more uniform.
[0073] In this embodiment, by mass percentage, the silicon oxide is 15%-25%, the aluminum oxide is 20%-30%, the diatomaceous earth is 2%-8%, the pore former is 10%-25%, and the glass powder is 20%-30%. This embodiment also provides an optimal ratio scheme for the above components. By adopting the content ratio provided in this embodiment, the above raw materials can be matched with each other to further prepare a porous ceramic atomizer core with low sintering temperature, small shrinkage, high strength, high porosity, and uniform pore size, thereby improving the service life of a large-capacity atomizer.
[0074] Please refer to Figure 3 , Figure 3 This is a schematic diagram of the three-dimensional structure of an atomizer core provided in an embodiment of the present application. This embodiment provides an atomizer core 1, which is composed of an atomizer core substrate 10 and a heating sheet 20. The atomizer core 1 is prepared by the preparation method of the atomizer core 1 provided in the above embodiment of the present application, which can reduce the sintering temperature during the sintering process, reduce the shrinkage rate of the atomizer core 1, and improve the structural strength of the atomizer core 1.
[0075] In summary, the present application provides a low-temperature glass powder and a preparation method thereof, as well as a low-temperature porous ceramic atomizer core 1 and a preparation method thereof. By making the glass powder have the characteristics of low softening point, low expansion coefficient and high strength, a porous ceramic atomizer core 1 with low sintering temperature, small shrinkage rate, high strength, high porosity and uniform pore size can be prepared.
[0076] In the description of the present application, it is necessary to understand that the terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise" and the like to indicate orientations or positional relationships are based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present application and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present application.
[0077] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Thus, a feature defined as "first" or "second" may explicitly or implicitly include one or more of the features. In the description of this application, the meaning of "plurality" is two or more, unless otherwise clearly and specifically defined. In addition, the terms "including" and "having" and any variations thereof are intended to cover non-exclusive inclusions.
[0078] In this application, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense, for example, it can be connected, detachably connected, or integrated. It can be mechanically connected or electrically connected. It can be directly connected or indirectly connected through an intermediate medium, and it can be the internal connection of two elements or the interaction relationship between two elements. For ordinary technicians in this field, the specific meanings of the above terms in this application can be understood according to the specific circumstances.
[0079] The above describes the contents provided by the implementation methods of the present application in detail, and describes and illustrates the principles and implementation methods of the present application. These explanations are only used to help understand the method and its core ideas of the present application. However, the contents of this specification should not be construed as limiting the present application, and those skilled in the art may make various changes and modifications to the present application without departing from the spirit and scope of the present application. These modifications and variations of the present application fall within the scope of the claims of the present application and their equivalents.
Claims
1. A glass powder, characterized in that: The glass powder includes silicon oxide, a main softener, and a secondary softener. The main softener includes at least one of boron oxide, zinc oxide, and bismuth oxide. The secondary softener includes at least one of potassium oxide and lithium oxide.
2. The glass powder according to claim 1, characterized in that In terms of mass percentage, the silicon oxide is 5%-10%, the boron oxide is 35%-50%, the zinc oxide is 10%-20%, the bismuth oxide is 20%-40%, the potassium oxide is 0%-5%, and the lithium oxide is 0%-5%.
3. A method for preparing glass powder, characterized in that: The preparation method comprises: Providing silicon oxide, a main softener, and a secondary softener, wherein the main softener includes at least one of boron oxide, zinc oxide, and bismuth oxide, and the secondary softener includes at least one of potassium oxide and lithium oxide; The silicon oxide, the main softener, and the secondary softener are uniformly mixed and dried to obtain a mixture; Melting the mixed material to obtain a molten liquid, and quenching the molten liquid to obtain a glass material; The glass material is crushed, ball-milled, dried and sieved in sequence to obtain glass powder.
4. A method for preparing an atomizer core, characterized in that: The preparation method comprises: Providing a solute and a solvent, wherein the solute comprises a matrix material, a pore former, and the glass powder according to any one of claims 1 to 2; The solute is dried, and the dried solute and the solvent are treated with wax to obtain a mixed slurry; Providing a heating sheet, processing the mixed slurry and the heating sheet through a slip injection molding process, so that the mixed slurry forms an atomizer core matrix embryo, and fixing the heating sheet to the atomizer core matrix embryo, to obtain an atomizer core embryo; The atomizer core embryo is processed through a degreasing process and a sintering process to obtain an atomizer core.
5. The preparation method according to claim 4, characterized in that: In the sintering process, the maximum sintering temperature is no more than 600°C.
6. The preparation method according to claim 4, characterized in that: The matrix material includes silicon oxide, aluminum oxide, and diatomaceous earth.
7. The preparation method according to claim 6, characterized in that: The particle size of the silicon oxide is 18-24 μm, the particle size of the aluminum oxide is 30-35 μm, and the particle size of the diatomaceous earth is 2-6 μm.
8. The preparation method according to claim 7, characterized in that: The particle size of the pore-forming agent is 50-70 μm.
9. The preparation method according to claim 6, characterized in that: In terms of mass percentage, the silicon oxide accounts for 15%-25%, the aluminum oxide accounts for 20%-30%, the diatomaceous earth accounts for 2%-8%, the pore-forming agent accounts for 10%-25%, and the glass powder accounts for 20%-30%.
10. An atomizer core, characterized in that: The atomizer core is prepared by the atomizer core preparation method according to any one of claims 4 to 9.