Negative carbon aggregate prepared by combining alkali excitation and carbonization and method thereof

Through the combination of carbonized gelling materials, alkali excitation materials and auxiliary gelling materials, the preparation method of alkali excitation and carbonization is adopted to solve the problems of poor strength and stability in the early stage of alkali excitation gelling materials, forming high-strength and stable negative Carbon aggregate is suitable for high-heat environments and realizes resource utilization of waste.

CN118908602APending Publication Date: 2024-11-08山东京韵泰博负碳科技有限公司
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411251976.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-09
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing alkali-excited gelling materials have poor strength in the early stage, easy cracking when they are dried and shrink, and poor stability of carbon mineralized materials.

Method used

Through the combination of carbonized gelling materials, alkali excitation materials and auxiliary gelling materials, the proportion and performance of gelling materials are adjusted, and the preparation method of alkali excitation and carbonization is used to form high-strength carbon negative aggregates, including carbonized gellings Mixed slurry forming and natural and carbonization curing processes of coagulation materials, alkali-exciting materials and auxiliary gelling materials.

Benefits of technology

It significantly improves the compressive strength and stability of the aggregate, isolates the reaction between CaCO3 and H2O and CO2, ensures the stability of CaCO3, and realizes the resource utilization of solid waste, adapts to the application of high-thermal environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005032705040000041
    Figure BDA0005032705040000041
  • Figure BDA0005032705040000042
    Figure BDA0005032705040000042
  • Figure BDA0005032705040000043
    Figure BDA0005032705040000043
Patent Text Reader

Abstract

The invention relates to the technical field of carbon mineralization materials and products, in particular to a negative carbon aggregate prepared through combination of alkali excitation and carbonization and a preparation method of the negative carbon aggregate. The negative carbon aggregate comprises a carbonized cementing material, an alkali-activated material and an auxiliary cementing material, the alkali-activated material accounts for 3%-7% of the mass of the carbonized cementing material, and the auxiliary cementing material accounts for 5%-15% of the mass of the carbonized cementing material. The preparation method comprises the following steps: fully stirring and mixing a carbonized cementing material, an alkali-activated material, an auxiliary cementing material and water to obtain mixed slurry, molding the mixed slurry, and carrying out natural curing and carbonization treatment to prepare the negative carbon aggregate. And the strength of the product is obviously improved by adjusting the ratio of the cementing material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of carbon mineralization materials and products, and more specifically, to a negative carbon aggregate prepared by combining alkali excitation and carbonization and a method thereof. Background Art

[0002] Alkali-activated cementitious materials, also known as "chemically activated cementitious materials", are hydraulic cementitious materials made by the catalytic principle of alkali activators (caustic alkali, alkali-containing silicates, aluminates). They include alkali-slag cement, geopolymer or geopolymer cement, etc. They are mainly composed of calcined natural minerals or industrial waste residues containing aluminum silicates with certain rapid cooling and heating phenomena (such as metakaolin, slag, fly ash, silica fume, steel slag, etc.) and alkali activators. They have the characteristics of fast coagulation and hardening, high strength and high temperature resistance. However, they will also show obvious drying shrinkage and cracking. If the product is prepared according to the above-mentioned alkali-activated materials, it will definitely lead to the problem of unbalanced application of product raw materials, that is, the raw materials cannot play their roles to the greatest extent. For example, patent CN111454011B discloses a method for preparing alkali-activated cementitious materials using engineering slag and alkali-activated cementitious materials. The main disclosure is that the engineering slag is calcined to obtain calcined slag, the calcined slag is mixed with an alkali activator solution, and the polymer slurry obtained by the mixture is vibrated, cured at room temperature and wet cured in sequence, wherein the engineering slag is granite residual soil, and the granite residual soil includes 50wt.% quartz and 30-35wt.% kaolin; the raw materials contain free calcium, potassium and other elements, and these ions will react with the gelling substances therein after the gelling material absorbs moisture, so that the crystallization of calcium aluminum ore has more pores, which accelerates the precipitation of Ca(OH)2, thereby causing the strength to decrease. Therefore, the technical solution of this application adds other gelling phases and additives to make various materials fully play their roles, adjust the proportion and performance of the gelling material, and improve the strength of the product. Summary of the invention

[0003] In view of this, the purpose of the present invention is to provide a negative carbon aggregate prepared by combining alkali activation and carbonization and a method thereof. The present application prepares high-strength aggregate by combining carbonized cementitious materials, alkali activated materials, and auxiliary cementitious materials to solve the problems of poor early strength of ordinary alkali activated materials, easy cracking due to drying shrinkage, and poor stability of carbon mineralized materials.

[0004] The invention provides a negative carbon aggregate prepared by combining alkali activation and carbonization. The negative carbon aggregate comprises: a carbonized cementitious material, an alkali activated material, and an auxiliary cementitious material.

[0005] The carbonized gelling material of the present invention is a substance containing monocalcium silicate, dicalcium silicate, tricalcium disilicate and the like which can produce carbonized gelling effect, such as one or more of steel slag, magnesium slag, furnace slag, carbide slag and the like.

[0006] The alkali-activated material accounts for 3%-7% of the mass fraction of the carbonized gelled material.

[0007] The alkali-activated materials are sodium phosphate and sodium sulfate. In addition, water glass, sodium carbonate, sodium hydroxide, potassium water glass, potassium phosphate, potassium carbonate, potassium sulfate, etc. with a modulus of 1.2-1.6 can also be selected.

[0008] The auxiliary gelling material accounts for 5%-15% of the mass fraction of the carbonized gelling material.

[0009] The auxiliary cementitious material is a high-activity silicon-aluminum material such as granulated blast furnace slag, mineral powder, fly ash, etc.

[0010] The present invention also provides a method for preparing negative carbon aggregate by combining alkali excitation and carbonization, the preparation method comprising:

[0011] Step 1: Prepare slurry, take carbonized gelling material, 3%-7% alkali activated material and 5%-15% auxiliary gelling material according to the ratio, add water and mix evenly;

[0012] Step 2: Forming, slurry forming to prepare aggregate;

[0013] Step 3: Natural curing: after pouring, natural curing at normal temperature and pressure;

[0014] Step 4: Carbonation curing: curing is carried out under carbon dioxide conditions to obtain high-strength aggregate prepared by combining alkali excitation and carbonization.

[0015] The molding described in the present invention includes but is not limited to common artificial aggregate molding methods such as casting molding, extrusion molding, roll molding, and granulator molding.

[0016] In step three of the present invention, the natural curing time is 24-72 hours, the curing temperature is 20-30 degrees Celsius, and the curing humidity is 35%-80%.

[0017] The carbonization curing conditions of the present invention are as follows: the volume concentration of carbon dioxide is greater than 5%, the carbonization pressure is 0.01-1 MPa, and the carbonization time is 18-30 hours.

[0018] The technical solution provided by the present invention has the following positive effects:

[0019] The present invention provides a negative carbon aggregate prepared by combining alkali excitation and carbonization and a method thereof. In the scheme, the silicon-aluminum amorphous spatial network structure formed by the reaction of alkali and active materials can improve the strength of the aggregate and isolate CaCO3 from reacting with H20 and CO2, thereby ensuring the stability of CaCO3. The aggregate prepared by combining alkali excitation and carbonization according to the technical scheme has been subjected to a boiling resistance test, and the strength is significantly improved.

[0020] (1) The activator, carbonized cementitious material and other auxiliary cementitious materials assist each other. By adjusting the proportion and performance of the cementitious materials, the strength of the product can be significantly improved.

[0021] (2) The product adopts a combination of alkali excitation and carbonization, which can make use of a large amount of solid waste and achieve the purpose of waste resource utilization.

[0022] (3) The aggregate prepared by the present invention has a dense structure and the cementitious phases are tightly connected. It not only has a wide range of applications but also a variety of application scenarios and can also adapt to high-temperature environments. BRIEF DESCRIPTION OF THE DRAWINGS DETAILED DESCRIPTION

[0023] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. The technical solution of the present application is further explained based on the embodiments of the present invention, which is not intended to limit the present invention and all other embodiments obtained by ordinary technicians in the field without creative work also belong to the technical scope protected by the present invention.

[0024] The present invention is further described in detail through the following examples, and the raw materials in the examples and comparative examples of the present application are calculated by weight, and the test raw materials and reagents involved are commonly available on the market.

[0025] The test methods or standards involved in the present invention are:

[0026] Compressive performance: tested in accordance with the standard JG / T568-2019 "Aggregates for High Performance Concrete".

[0027] Specific Examples 1-5 and Comparative Example 1

[0028] The negative carbon aggregate prepared by combining alkali activation and carbonization in an embodiment of the present invention includes: 100 parts of carbonized cementitious material (to avoid redundancy, steel slag is taken as an example here), the alkali-activated material is added in an amount of 3%-7% of the mass of the carbonized cementitious material (preferably 3 parts, 4 parts, 5 parts, 6 parts, 7 parts), and the auxiliary cementitious material is added in an amount of 5%-15% of the mass of the carbonized cementitious material (preferably 5 parts, 7.5 parts, 10 parts, 12.5 parts, 15 parts). The carbonized cementitious material, alkali-activated material, auxiliary cementitious material and water are fully stirred and mixed to obtain a mixed slurry, the mixed slurry is molded, and carbonization treatment is carried out after natural curing for a certain period of time, and the compressive properties are tested according to JG / T568-2019 "Aggregates for High Performance Concrete"; then the boiling resistance of the aggregate is tested, and the specific operating steps are as follows: the prepared aggregate is boiled in boiling water for 3 hours, then taken out and the compressive strength is tested according to JG / T568-2019 "Aggregates for High Performance Concrete", and the stability of the aggregate is considered according to the loss rate of the compressive strength value.

[0029] Examples and Comparative Examples

[0030]

[0031] Performance Test Results

[0032]

[0033]

[0034] Result analysis:

[0035] Comparison between Comparative Example 1 and Examples 1-5 shows that the comparative example uses carbonized cementitious material to prepare aggregate, and its compressive strength after carbonization is too small at 3 days, and it is difficult for the testing equipment to detect the strength value, and the compressive strength at 7 days is only 7 MPa.

[0036] It can be seen from Examples 1-5 that the aggregates provided by the technical solution of the present invention have a 3-day compressive strength of 33MP-46MPa. This is because the present invention adopts a combined method of alkali activation and carbonization to prepare negative carbon aggregates, wherein the silicon-aluminum amorphous spatial network structure formed by the reaction of alkali and active materials can improve the strength of the aggregate, while isolating CaCO3 from reacting with H20 and CO2 to ensure the stability of CaCO3; and through the boiling resistance test, it is shown that the strength is significantly improved, which is because the interaction between the carbonized cementitious material and the alkali-activated material and the auxiliary cementitious material in the aggregate during the boiling process is optimized, thereby improving the overall strength of the aggregate.

[0037] It can be seen from Examples 1-5 that aggregate can be prepared by formulas in which the alkali-activated material accounts for 3%-7% of the carbonized cementitious material and the auxiliary cementitious material accounts for 5%-15% of the carbonized cementitious material. Therefore, this range of values ​​is the preferred range of the present technical solution. Through comprehensive evaluation of compressive strength and strength loss rate, it can be seen that the performance indicators of the alkali-activated material accounting for 4%-5% of the carbonized cementitious material and the auxiliary cementitious material accounting for 7%-10% of the carbonized cementitious material are particularly ideal. This is because the activator, the carbonized cementitious material and other auxiliary cementitious materials assist each other. By adjusting the ratio and performance of the cementitious material, the strength of the product is significantly improved, and the overall cost is also low, which is more suitable for industrial production.

[0038] The specific embodiments of the present invention described above do not constitute the scope of protection of the present invention, but are to comply with the widest scope consistent with the principles and novel features disclosed herein. Therefore, any corresponding adjustments made based on the technical concept of the present invention should be included in the scope of protection of the claims of the present invention.

Claims

1. A negative carbon aggregate prepared by combining alkali activation and carbonization, characterized in that: The negative carbon aggregate comprises: carbonized cementitious material, alkali-activated material and auxiliary cementitious material.

2. The negative carbon aggregate prepared by combining alkali activation and carbonization according to claim 1, characterized in that: The carbonized gelling material is a substance containing components such as monocalcium silicate, dicalcium silicate, and tricalcium disilicate, which can produce carbonized gelling effect.

3. The negative carbon aggregate prepared by combining alkali activation and carbonization according to claim 1, characterized in that: The alkali-activated material accounts for 3%-7% of the mass fraction of the carbonized gelled material.

4. The negative carbon aggregate prepared by combining alkali activation and carbonization according to claim 3, characterized in that: The alkali excitation materials are sodium phosphate and sodium sulfate.

5. The negative carbon aggregate prepared by combining alkali activation and carbonization according to claim 4, characterized in that: The alkali-activated material may also be selected from water glass, sodium carbonate, sodium hydroxide, potassium water glass, potassium phosphate, potassium carbonate, potassium sulfate, etc., with a modulus of 1.2-1.

6.

6. The negative carbon aggregate prepared by combining alkali activation and carbonization according to claim 1, characterized in that: The auxiliary gelling material accounts for 5%-15% of the mass fraction of the carbonized gelling material.

7. The negative carbon aggregate prepared by combining alkali activation and carbonization according to claim 6, characterized in that: The auxiliary cementitious material is a high-activity silicon-aluminum material such as granulated blast furnace slag, mineral powder, fly ash, etc.

8. A method for preparing negative carbon aggregate by combining alkali excitation and carbonization, characterized in that: The preparation method comprises: Step 1: Prepare slurry, take carbonized gelling material, alkali activated material and auxiliary gelling material according to the ratio, add water and mix evenly; Step 2: Forming, slurry forming to prepare aggregate; Step 3: Natural curing: after pouring, natural curing at normal temperature and pressure; Step 4: Carbonation curing: curing is carried out under carbon dioxide conditions to obtain high-strength aggregate prepared by combining alkali excitation and carbonization.

9. The method for preparing negative carbon aggregate by combining alkali excitation and carbonization according to claim 8, characterized in that: In step three of the present invention, the natural curing time is 24-72 hours, the curing temperature is 20-30 degrees Celsius, and the curing humidity is 35%-80%.

10. The method for preparing negative carbon aggregate by combining alkali excitation and carbonization according to claim 8, characterized in that: The carbonization curing conditions are as follows: the volume concentration of carbon dioxide is greater than 5%, the carbonization pressure is 0.01-1 MPa, and the carbonization time is 18-30 hours.

Citation Information

Cited By

  • All-solid-waste two-stage carbon sequestration alkali-activated geopolymer concrete and preparation method thereof

    CN122325160A