Artificial fine stone aggregate as well as preparation method and application thereof
By using concrete residues as the core of artificial fine stone aggregate and encapsulating them in ultra-high concrete leather, environmental pollution and resource waste caused by landfill of concrete production waste slag is solved, efficient utilization and strength improvement are achieved, and the engineering application is met. Carrying capacity requirements.
Patent Information
- Application Number
- CN202410954592.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-11-08
AI Technical Summary
In the prior art, most of the waste slag produced during concrete production is directly landfilled, resulting in environmental pollution and waste of resources, and the consumption of resources and energy increases, and the pollution problem is becoming increasingly serious.
Concrete residues are used as the core of artificial fine stone aggregate, and are packaged through ultra-high concrete leather to prepare artificial fine stone aggregates with high bearing strength. They are prepared by mixing and granulation technology, and exciters and silicon are added. The ash and cement are activated to improve the strength of the aggregate.
The reuse of concrete residues has been achieved, environmental pollution has been reduced, natural resources have been saved, and the load-bearing strength of artificial fine stone aggregates has reached 2.50~2.70MPa, meeting the engineering usage requirements.
Smart Images

Figure CN118908608A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of construction waste recycling, and in particular relates to an artificial fine stone aggregate and a preparation method and application thereof. Background Art
[0002] At present, the annual use of concrete exceeds 4 billion cubic meters, and the use of aggregates exceeds 6 billion tons. There is a huge demand for aggregates, which leads to a large amount of quarrying and damages the ecological environment. As the environmental, economic and social problems caused by the reduction of global resources become increasingly prominent, more and more attention is paid to energy conservation and resource recycling, and waste reuse is vigorously advocated and developed.
[0003] With the huge concrete production, resource and energy consumption has soared, and the pollution has also increased. There are many kinds of pollution generated when commercial concrete mixing plants produce concrete, mainly dust pollution in the air, water pollution when cleaning equipment, sound pollution generated by the mixing station during production, and residual concrete waste. In the prior art, most of the produced concrete waste is usually directly discharged and landfilled, which not only pollutes the environment but also causes a waste of resources. Summary of the invention
[0004] The object of the present invention is to provide an artificial fine stone aggregate and a preparation method and application thereof. The artificial fine stone aggregate provided by the present invention is prepared by using concrete residues, thereby realizing the reuse of concrete residues, saving natural resources and reducing environmental pollution.
[0005] In order to achieve the purpose of the present invention, the present invention provides the following technical solutions:
[0006] An artificial fine stone aggregate comprises a concrete residue inner core and a super-high concrete skin covering the surface of the concrete residue inner core.
[0007] Preferably, the particle size of the concrete residue inner core is 4 to 20 mm; and the thickness of the super-high concrete skin material is 1 to 2 mm.
[0008] Preferably, the mass ratio of the concrete residue inner core to the ultra-high concrete skin material is 6-8:2-4.
[0009] Preferably, the concrete residue kernel comprises the following raw materials in mass fractions: 53-55% concrete residue, 10-12% activator and 33-36% water.
[0010] Preferably, the mass content of Ca(OH)2 in the concrete residue is 10 to 20 wt.%.
[0011] Preferably, the activator comprises petroleum coke residue, mineral powder and metakaolin; the mass ratio of the petroleum coke residue, mineral powder and metakaolin is 16-17:66-67:16-17.
[0012] Preferably, the ultra-high concrete skin material includes the following raw materials in parts by weight: 967-970 parts of cement, 107-110 parts of silica fume, 27-28 parts of water reducer and 193-195 parts of water.
[0013] The present invention also provides a method for preparing the artificial fine stone aggregate described in the above technical solution, comprising the following steps:
[0014] The raw materials for preparing the concrete residue core are first mixed and then granulated to obtain the concrete residue core;
[0015] The raw materials for preparing the super-high concrete skin material are mixed for the second time to obtain super-high concrete slurry;
[0016] The concrete residue core and the superconcrete slurry are mixed for the third time and cured to obtain the artificial fine stone aggregate.
[0017] Preferably, the first mixing, the second mixing and the third mixing are performed by stirring; the stirring mixing rate is 120-125 r / min;
[0018] The granulation rate is 40-60 r / min.
[0019] The present invention also provides the use of the artificial fine stone aggregate described in the above technical solution or the artificial fine stone aggregate prepared by the preparation method described in the above technical solution in concrete.
[0020] The present invention provides an artificial fine stone aggregate, comprising a concrete residue inner core and an ultra-high concrete skin coated on the surface of the concrete residue inner core. The present invention uses concrete residue as the main component of the artificial fine stone aggregate inner core, realizes the reuse of concrete residue, saves natural resources, and reduces environmental pollution. At the same time, the ultra-high concrete skin encapsulates the concrete residue inner core, so that the bearing capacity strength of the artificial fine stone aggregate meets the engineering use (Standard for Quality and Inspection Methods of Sand and Stone for Ordinary Concrete JGJ52-2006). Furthermore, the present invention activates the concrete residue by adding an activator, silica fume and cement, thereby further improving the bearing capacity strength of the artificial fine stone aggregate. It can be seen from the results of the embodiments of the present invention that the single-particle bearing capacity strength of the artificial fine stone aggregate is 2.50 to 2.70 MPa. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.
[0022] Figure 1 This is a diagram of the preparation process of the artificial fine stone aggregate of the present invention;
[0023] Figure 2 It is a schematic diagram of the structure of the artificial fine stone aggregate of the present invention. DETAILED DESCRIPTION
[0024] The invention provides an artificial fine stone aggregate, comprising a concrete residue inner core and a super-high concrete skin material covering the surface of the concrete residue inner core.
[0025] In the present invention, the particle size of the concrete residue core is preferably 4-20 mm, more preferably 8-10 mm; the thickness of the super-high concrete skin is preferably 1-2 mm. In the present invention, the mass ratio of the concrete residue core to the super-high concrete skin is preferably 6-8:2-4, more preferably 6:4.
[0026] In the present invention, the concrete residue core preferably includes the following raw materials by mass: 53-55% concrete residue, 10-12% activator and 33-36% water.
[0027] In the present invention, the raw materials for preparing the concrete residue inner core preferably include 53-55% concrete residue, more preferably 54% by mass. In the present invention, the mass content of Ca(OH)2 in the concrete residue is preferably 10-20wt.%. In the present invention, the concrete residue preferably includes hydrated cement and unhydrated cement. In the present invention, the mass ratio of the cement to the unhydrated cement is preferably 3-7:1-3, more preferably 3:1.
[0028] In the present invention, the concrete residue is preferably obtained by treating the concrete waste residue produced by the mixing station in a multi-stage sedimentation tank to obtain a sedimentation slurry; the waste residue 10 cm below the surface of the sediment in the sedimentation slurry is shoveled, and then dried to stop its hydration reaction. In the present invention, the drying temperature is preferably 60-80°C, and the time is preferably 6-8h.
[0029] In the present invention, the raw materials for preparing the concrete residue kernel preferably include 10-12% of the activator, more preferably 11% by mass fraction. In the present invention, the activator preferably includes petroleum coke slag, mineral powder and metakaolin. In the present invention, the mass ratio of the petroleum coke slag, mineral powder and metakaolin is preferably 12-16:65-67:12-16. In the present invention, the activator has the function of stimulating the activity of the concrete waste residue.
[0030] In the present invention, the raw materials for preparing the concrete residue inner core preferably include 33-36% water, more preferably 35% by mass. In the present invention, the water is preferably distilled water.
[0031] In the present invention, the ultra-high concrete skin material preferably includes the following raw materials in parts by weight: 967-970 parts of cement, 107-110 parts of silica fume, 27-28 parts of water reducer and 193-195 parts of water.
[0032] In the present invention, the raw materials for preparing the ultra-high concrete skin material preferably include cement 967-970 by mass. In the present invention, the cement is preferably 525 Conch Cement.
[0033] In the present invention, the raw materials for preparing the ultra-high concrete skin material preferably include 107-110 parts of silica fume by weight. In the present invention, the particle size of the silica fume is preferably 800-1000 mesh; the mass content of SiO2 in the silica fume is preferably 92wt.%. In the present invention, the silica fume has the function of filling the tiny pores inside the aggregate, improving the density of the aggregate and thus enhancing the strength of the artificial aggregate.
[0034] In the present invention, the raw materials for preparing the ultra-high concrete skin material preferably include 27 to 28 parts of a water reducer by weight. In the present invention, the water reducer is preferably a polycarboxylic acid high-performance water reducer.
[0035] In the present invention, the raw materials for preparing the ultra-high concrete skin material preferably include 193 to 195 parts of water by weight. In the present invention, the water is preferably distilled water.
[0036] In the present invention, the raw materials for preparing the super-high concrete skin material preferably further include a defoamer; the dosage of the defoamer is 0.01-0.02wt% of the super-high concrete skin material.
[0037] In the present invention, the particle size of the artificial fine stone aggregate is preferably 4-20 mm, more preferably 10-15 mm; the single particle bearing strength of the artificial fine stone aggregate is preferably 2.50-2.70 MPa, more preferably 2.53-2.68 MPa, further preferably 2.61-2.65 MPa.
[0038] The present invention also provides a method for preparing the artificial fine stone aggregate described in the above technical solution, comprising the following steps:
[0039] The raw materials for preparing the concrete residue core are first mixed and then granulated to obtain the concrete residue core;
[0040] The raw materials for preparing the super-high concrete skin material are mixed for the second time to obtain super-high concrete slurry;
[0041] The concrete residue core and the superconcrete slurry are mixed for the third time and cured to obtain the artificial fine stone aggregate.
[0042] The present invention performs a first mixing of the raw materials for preparing the concrete residue inner core, and then performs granulation to obtain the concrete residue inner core. In the present invention, it is preferred to first mix the concrete residue, cement, silica fume and activator to obtain a mixed dry material, and then perform granulation, and spray water during the granulation process to obtain the concrete residue inner core. In the present invention, the first mixing method is preferably stirring and mixing. In the present invention, the stirring and mixing rate is preferably 110 to 120 r / min. The present invention does not specifically limit the stirring and mixing time, as long as the purpose of uniform mixing is achieved.
[0043] In the present invention, the granulation is preferably carried out in a disc granulator. In the present invention, the rotation speed of the granulation is preferably 40 to 60 r / min.
[0044] In the present invention, the granulation is preferably followed by carbonization. In the present invention, the carbonization temperature is preferably 18-24°C, the relative humidity is preferably 55-65%, the time is preferably 24-48h; and the mass fraction of carbon dioxide is preferably 20-22wt.%.
[0045] The present invention performs a second mixing of the raw materials for preparing the superconcrete skin material to obtain the superconcrete slurry. In the present invention, the second mixing is preferably consistent with the first mixing method, which will not be repeated here.
[0046] The present invention performs a third mixing of the concrete residue core and the ultra-high concrete slurry, and obtains the artificial fine stone aggregate after curing. In the present invention, the third mixing is preferably consistent with the first mixing method, which will not be described in detail here.
[0047] In the present invention, the curing is preferably standard curing; the curing temperature is preferably 20-22° C., the relative humidity is preferably 90-95%, and the curing time is preferably 7-14 days, more preferably 10-12 days.
[0048] The present invention also provides the use of the artificial fine stone aggregate described in the above technical solution in concrete.
[0049] In the present invention, the amount of the artificial fine stone aggregate in the concrete is preferably 20-30 wt.%, more preferably 25-28 wt.%, based on the total mass of the concrete.
[0050] In order to further illustrate the present invention, the artificial fine stone aggregate provided by the present invention is described in detail below in conjunction with the accompanying drawings and embodiments, but they should not be construed as limiting the protection scope of the present invention.
[0051] Example 1
[0052] The concrete residue was placed in a granulator according to the proportion described in Table 1. According to the water-cement ratio of the concrete residue and water being 0.46, water was sprayed into the granulator in a mist form using a spray pot. At a rotation speed of 40 r / min, a concrete residue inner core with a particle size of 4 to 10 mm was prepared. The core was allowed to stand for 6 hours, and carbonized and cured for 24 hours under the conditions of 20 to 22 wt.% CO2 and 65% relative humidity at room temperature, and the single aggregate compressive bearing capacity of the concrete residue inner core was tested.
[0053] Table 1 Ratio of raw materials of concrete residue kernel in Example 1
[0054]
[0055] Table 1 explores the effect of the standing time of concrete waste (i.e., the Ca(OH)2 content in the concrete residue after hydration) on the strength of artificial fine stone aggregate. It can be seen from Table 1 that the longer the standing time of the concrete residue, that is, the longer the hydration reaction time, the lower the internal Ca(OH)2 content, resulting in lower strength of the artificial fine stone aggregate.
[0056] Example 2
[0057] Concrete residue and activator (10.75 g of petroleum coke residue, 43.5 g of mineral powder and 10.75 g of metakaolin) were placed in a granulator according to the proportion described in Table 2. According to the water-cement ratio of concrete residue and water being 0.46, water was sprayed into the granulator in a mist form using a spray pot. At a speed of 40 r / min, a concrete residue inner core with a particle size of 4 to 10 mm was prepared. The core was allowed to stand for 6 hours, and carbonized and cured for 24 hours under the conditions of 20 to 22 wt.% of CO2 and 65% relative humidity at room temperature, and the single aggregate compressive bearing capacity of the concrete residue inner core was tested.
[0058] Table 2 Ratio of raw materials of concrete residue kernel in Example 2
[0059]
[0060]
[0061] It can be seen from the results in Table 2 that the core of the concrete residue to which the activator of the present invention is added has a higher strength.
[0062] Example 3
[0063] according to Figure 1 The process diagram is used to prepare artificial fine stone aggregate. The UHPC slurry is mixed according to the ratio described in Table 3 and fully stirred using a planetary mixer to obtain a slurry. The concrete residue kernels prepared in Example 1 and Example 2 are poured into the slurry and placed on a vibrating table so that the concrete residue kernels are evenly wrapped by the slurry. A colander with an aperture size of 5 to 8 mm is used to fish out the evenly wrapped aggregates. The excess slurry is removed by the vibration effect of the vibrating table. After curing for 12 hours under natural conditions, the aggregates are transferred to a standard curing room for curing for 7 days to obtain artificial fine stone aggregate.
[0064] Table 3 UHPC leather raw material ratio
[0065] raw material Silica fume(g) Cement(g) Water(g) Water reducing agent(g) UHPC 107 967 193 27
[0066] The single particle bearing strength of the artificial fine stone aggregate described in Example 3 was tested, and the test results are shown in Table 4.
[0067] Table 4 Example 3 Single particle bearing strength test results of artificial fine stone aggregate
[0068] Sources of artificial fine stone aggregate Single particle bearing strength (MPa) Example 1-L1 2.50 Example 1-L2 2.61 Example 2-J1 2.53 Example 2-J2 2.65
[0069] Figure 2 It is a schematic diagram of the structure of the artificial fine stone aggregate of the present invention.
[0070] From the results in Table 4, it can be seen that the UHP concrete shell significantly improves the strength of artificial aggregate.
[0071] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. People can also obtain other embodiments based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.
Claims
1. An artificial fine stone aggregate, It is characterized in that It comprises a concrete residue inner core and an ultra-high performance concrete skin material coated on the surface of the concrete residue inner core.
2. The artificial fine stone aggregate according to claim 1, It is characterized in that The particle size of the concrete residue inner core is 4 to 20 mm; the thickness of the super-high concrete skin material is 1 to 2 mm.
3. The artificial fine stone aggregate according to claim 1 or 2, It is characterized in that The mass ratio of the concrete residue inner core to the ultra-high concrete skin material is 6-8:2-4.
4. The artificial fine stone aggregate according to claim 1, It is characterized in that The concrete residue kernel comprises the following raw materials in mass fractions: 53-55% of concrete residue, 10-12% of activator and 33-36% of water.
5. The artificial fine stone aggregate according to claim 4, It is characterized in that The Ca(OH) in the concrete residue 2 The mass content is 10 to 20 wt.%.
6. The artificial fine stone aggregate according to claim 4, It is characterized in that The activator comprises petroleum coke residue, mineral powder and metakaolin; the mass ratio of the petroleum coke residue, mineral powder and metakaolin is 16-17:66-67:16-17.
7. The artificial fine stone aggregate according to claim 1, It is characterized in that The ultra-high concrete skin material comprises the following raw materials in parts by weight: 967-970 parts of cement, 107-110 parts of silica fume, 27-28 parts of water reducing agent and 193-195 parts of water.
8. A method for preparing the artificial fine stone aggregate according to any one of claims 1 to 7, It is characterized in that The following steps are involved: The raw materials for preparing the concrete residue core are first mixed and then granulated to obtain the concrete residue core; The raw materials for preparing the super-high concrete skin material are mixed for the second time to obtain super-high concrete slurry; The concrete residue core and the superconcrete slurry are mixed for the third time and cured to obtain the artificial fine stone aggregate.
9. The preparation method according to claim 8, It is characterized in that The first mixing, the second mixing and the third mixing are performed by stirring and mixing; the stirring and mixing speed is 120 to 125 r / min; The granulation rate is 40-60 r / min.
10. Use of the artificial fine stone aggregate according to any one of claims 1 to 7 or the artificial fine stone aggregate prepared by the preparation method according to claim 8 or 9 in concrete.