Composite material prepared from tuff powder waste and preparation method thereof

By mixing tuff rock powder and granulated blast furnace slag powder with alkali liquid to form a gel, the problem of tuff rock powder waste utilization is solved, and the preparation of high-performance composite materials is realized, which reduces costs and increases compressive strength.

CN118908636APending Publication Date: 2024-11-08LANZHOU UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411007962.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The prior art is difficult to effectively utilize tuff rock powder waste, and the alkali excitation method is used to high cost, affecting material performance, and lacking a low-cost preparation method without high-temperature calcination to form high-performance composite materials.

Method used

By mixing tuff rock powder, granulated blast furnace slag powder and alkali liquid in a certain proportion, a gel is formed, and the quartz and feldspar monomers are dissolved using high concentration of alkali liquid to reconstruct the three-dimensional space network polymerization gel, and silicon aluminum is used to dissolve silicon and aluminum. Acid minerals produce cementation to prepare green and low-carbon composite materials.

Benefits of technology

The resource utilization of tuff rock powder waste is realized, production costs are reduced, high-performance composite materials are formed, and they are suitable for different engineering needs, meeting the improvement of compressive strength.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118908636A_ABST
    Figure CN118908636A_ABST
Patent Text Reader

Abstract

The invention discloses a composite material prepared from tuff powder waste and a preparation method thereof. The preparation method comprises the following steps: uniformly mixing and stirring 10.00-11.67 parts of tuff stone powder waste and 5.00-6.67 parts of blast furnace slag powder, adding 33.40 parts of sand and 40.8 parts of gravel, and uniformly stirring to obtain a dry mixture; adding 9.13 parts of alkali liquor into the dry mixture, and uniformly stirring to obtain a mixture; and finally, pouring the mixture into a mold, vibrating, compacting and trowelling, covering the surface with a preservative film for sealing, curing in an oven at 80 DEG C for 24 hours, demolding, and curing a demolded test block in the oven environment to a set age to obtain the composite material. The invention has the advantages of greenness, environmental protection, simple process, low price and adjustable strength, and can meet the actual engineering requirements.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of development and utilization of building materials, and in particular relates to a composite material prepared from tuff stone powder waste and a preparation method thereof. Background Art

[0002] Tuff is a volcanic clastic rock with a tuff structure. It is mainly composed of quartz, feldspar and volcanic clastic components. It is a natural siliceous and aluminum raw material. Tuff, which is widely distributed, is also an important raw material for the production of artificial sand and gravel. In the process of dry production of artificial sand, stone powder accounting for about 20% of the total mass of artificial sand and gravel will be produced. However, there is currently a lack of effective recycling methods for these tuff stone powder wastes.

[0003] Previous studies have shown that using tuff rock powder waste to partially replace cement to prepare cementitious materials or concrete will reduce the compressive strength of the material, increase the number and diameter of internal pores, reduce the hydration rate, increase the shrinkage rate, and reduce workability. Using alkali-activated amorphous glassy geopolymers to form building materials is an important way to utilize solid waste. However, commonly used waste materials are mainly composed of fly ash, blast furnace slag, etc., which have been calcined at high temperatures, but the same alkali activation method is not applicable to tuff with better crystallinity. The alkali activators of alkali-activated materials are mainly NaOH and Na 2 SiO 3 However, too high Na 2 SiO 3 Affects economic efficiency. For example, the amount of water glass in the slurry of the disclosed invention patent "A fly ash-based polymer concrete material and its preparation method" (201410856420.X) is as high as 25%. The mass ratio of sodium silicate and sodium hydroxide used in the alkali activator of the disclosed invention patent "A high-performance geopolymer concrete and its preparation method" (202111287469.4) is as high as 2.8. Therefore, there is still a lack of a suitable preparation method that does not require high-temperature calcination of tuff and uses a low-cost alkali activator to form a high-performance tuff-based composite material. Summary of the invention

[0004] In order to overcome the shortcomings and deficiencies of the prior art, the object of the present invention is to provide a composite material prepared from tuff stone powder waste and a preparation method thereof.

[0005] The present invention is implemented as follows: a composite material prepared from tuff stone powder waste, the composite material comprises the following components by mass: 10.00-11.67 parts of tuff stone powder waste, 5.00-6.67 parts of blast furnace slag powder, 33.40 parts of sand, 40.8 parts of crushed stone, and 9.13 parts of alkali solution.

[0006] Preferably, the tuff stone powder waste is solid waste generated in the process of dry-process sand production, and its specific surface area is between 1100 and 1250 m 2 / kg, the particle size is above 350 mesh, the silicon dioxide content is greater than 40%, and the aluminum oxide content is greater than 12%.

[0007] Preferably, the blast furnace slag powder is S95 grade granulated blast furnace slag powder, and its specific surface area is 700-950m 2 / kg, the particle size is 1-120μm, the calcium oxide content is not less than 33%, and the aluminum oxide content is not higher than 15%.

[0008] Preferably, the sand is selected from one or more of natural sand, river sand and machine-made sand;

[0009] Preferably, the crushed stone is selected from one or more of tuff crushed stone, diabase crushed stone, granite crushed stone, basalt crushed stone, and recycled construction waste crushed stone.

[0010] Preferably, the sand is machine-made sand prepared from tuff, with an apparent density of 2.77 g / cm 3 The water absorption rate is 2.06% and the particle size is less than 5mm.

[0011] Preferably, the crushed stone is natural diabase crushed stone with an apparent density of 2300-3800 kg / m 3 The particle size range is 5 to 20 mm, the crushed stone with a particle size of 5 to 10 mm accounts for 20 to 26% of the total mass of the crushed stone, and the crushed stone with a particle size of 10 to 20 mm accounts for 74 to 80% of the total mass of the crushed stone.

[0012] Preferably, the alkali solution is selected from one or more of sodium hydroxide solution, potassium hydroxide solution and sodium silicate solution.

[0013] Preferably, the alkali solution is composed of a mixture of a sodium hydroxide solution with a volume concentration of 24% and a sodium silicate solution with a volume concentration of 2.0% in a volume ratio of 90.47:9.53.

[0014] The present invention further discloses a method for preparing the composite material, which comprises the following steps:

[0015] (1) mixing tuff stone powder waste and blast furnace slag powder evenly, adding sand and crushed stone and mixing evenly to obtain a dry mix;

[0016] (2) adding alkali solution to the dry mix and stirring evenly to obtain a mixture;

[0017] (3) Pour the mixture into a mold, vibrate and compact it, seal the surface with plastic wrap, and place it in an oven at 80°C for 24 hours. De-mold the demoulded test piece and cure it in the oven environment to the set age.

[0018] The present invention overcomes the deficiencies of the prior art and provides a composite material prepared from tuff stone powder waste and a preparation method thereof. The technical principle of the present invention is that by using a high concentration of alkali solution to dissolve its crystal structure, the Si and Al monomers of quartz and feldspar in the tuff stone powder waste are dissolved from the minerals, and a three-dimensional spatial network polymer gel can still be formed in the subsequent reconstruction and polycondensation process; at the same time, the siliceous coarse aggregate mainly plays a skeleton role in the composite material, which can limit the shrinkage of the system to a certain extent. At the same time, under the action of the high concentration of alkali solution in the system, the aluminosilicate minerals on the surface of the aggregate will also be slightly dissolved, producing a trace amount of geopolymer gel, which has a certain cementing effect. Based on the above principle, the present invention mixes tuff stone powder waste, granulated blast furnace slag powder, coarse and fine aggregates and alkali solution in a certain proportion to prepare a green and low-carbon composite material.

[0019] Compared with the shortcomings and deficiencies of the prior art, the present invention has the following beneficial effects:

[0020] (1) The present invention uses tuff stone powder waste generated in the process of machine-made sand production as the main material, and does not need to be calcined and ground, and is mixed with part of blast furnace slag powder as a gelling material, and forms a gel together through the action of alkali liquid, so the carbon footprint in the production process is small;

[0021] (2) The powder, machine-made sand and crushed stone used in the present invention are easily available and inexpensive, and the amount of sodium silicate solution used in the alkali solution is very small, which further reduces the preparation cost of the composite material of tuff stone powder waste and coarse aggregate;

[0022] (3) The present invention can prepare composite materials of different strengths by adjusting the system components, so that the prepared tuff stone powder waste and coarse aggregate composite materials are suitable for different engineering requirements;

[0023] (4) The preparation process of the composite material of the present invention is simple, and prefabricated blocks can be prepared and used, which provides a feasible solution for the resource utilization of solid waste tuff stone powder and the development of new low-carbon building materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 is the XRD diagram of the tuff rock powder waste and blast furnace slag powder used in the present invention;

[0025] Figure 2 It is a graph of the compressive strength of the composite material of the present invention. DETAILED DESCRIPTION

[0026] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.

[0027] The XRF analysis results of the tuff stone powder waste and blast furnace slag powder used in the following examples of the present invention are shown in Table 1, and the XRD analysis results are shown in Table 1. Figure 1 As shown:

[0028] Table 1 XRF analysis results of tuff stone powder waste and blast furnace slag powder

[0029] Oxide content / % Tuff stone powder waste Blast furnace slag powder <![CDATA[Al 2 THE 3 ]]> 16.36 13.82 <![CDATA[SiO 2 ]]> 40.50 34.63 <![CDATA[Na 2 The]]> 1.89 0.1 MgO 5.46 10.59 CaO 17.43 33.93 <![CDATA[K 2 The]]> 1.55 0.37 <![CDATA[Fe 2 THE 3 ]]> 14.75 0.28

[0030] Example 1

[0031] This embodiment is used to test the compressive properties of a composite material 1 containing 11.67% tuff stone powder waste and 5.00% blast furnace slag powder, which includes the following components in terms of mass percentage:

[0032] Tuff rock powder waste 11.67%, blast furnace slag powder 5.00%, machine-made sand 33.40%, 5-10mm aggregate 8.63%, 10-20mm aggregate 32.17%, 24% concentration sodium hydroxide solution 8.21%, 2% concentration sodium silicate solution 0.92%.

[0033] Tuff rock powder waste contains mineral components such as quartz, feldspar, calcite, chlorite, etc., with a particle size range of 0.35μm to 178.25μm, silicon dioxide (SiO 2 ) content is 40.50%, aluminum oxide (Al 2 O 3 ) content is 16.36%. Blast furnace slag powder is composed of amorphous aluminosilicates, with a particle size range of 1.00μm to 104.6μm, silicon dioxide (SiO 2 ) content is 33.93%, aluminum oxide (Al 2 O 3 ) content is 13.82%.

[0034] The preparation method of the composite material 1 comprises the following steps:

[0035] (1) 3.15 kg of tuff rock powder waste and 1.35 kg of blast furnace slag powder were mixed to form component A; 2.23 kg of sodium hydroxide solution and 0.25 kg of sodium silicate solution were mixed to form component B;

[0036] (2) After stirring component A for 2 minutes, 9 kg of machine-made sand, 2.31 kg of 5-10 mm aggregate, and 8.49 kg of 10-20 mm aggregate were added in sequence and stirred for 3 minutes to evenly disperse the aggregates;

[0037] (3) Component B is added and stirred for 3 minutes to obtain a composite material slurry consisting of tuff rock powder waste and coarse aggregate;

[0038] (4) The prepared composite material slurry was poured into a 100×100×100 mm mold twice, and vibrated on a vibration table for 1 to 2 minutes each time. After smoothing, it was covered with plastic wrap and placed in an oven at 80°C. The mold was removed after 24 hours, and the demolded test piece was directly placed in an oven environment for curing for a certain number of days to obtain a composite material 1.

[0039] Example 2

[0040] This embodiment is used to test the compressive properties of a composite material 2 containing 10.00% tuff stone powder waste and 6.67% blast furnace slag powder, which includes the following components in terms of mass percentage:

[0041] Tuff rock powder waste 10.00%, blast furnace slag powder 6.67%, machine-made sand 33.40%, 5-10mm aggregate 8.63%, 10-20mm aggregate 32.17%, 24% concentration sodium hydroxide solution 8.21%, 2% concentration sodium silicate solution 0.92%.

[0042] Tuff rock powder waste contains mineral components such as quartz, feldspar, calcite, chlorite, etc., with a particle size range of 0.35μm to 178.25μm, silicon dioxide (SiO 2 ) content is 40.50%, aluminum oxide (Al 2 O 3 ) content is 16.36%. Blast furnace slag powder is composed of amorphous aluminosilicate, with a particle size range of 0.97μm to 104.6μm, silicon dioxide (SiO 2 ) content is 33.93%, aluminum oxide (Al 2 O 3 ) content is 13.82%.

[0043] The preparation method of the composite material 2 comprises the following steps:

[0044] (1) 2.7 kg of tuff rock powder waste and 1.8 kg of blast furnace slag powder were mixed to form component A; 2.23 kg of sodium hydroxide solution and 0.25 kg of sodium silicate solution were mixed to form component B;

[0045] (2) After stirring component A for 2 minutes, 9 kg of machine-made sand, 2.31 kg of 5-10 mm aggregate, and 8.49 kg of 10-20 mm aggregate were added in sequence and stirred for 3 minutes to evenly disperse the aggregates;

[0046] (3) Component B is added and stirred for 3 minutes to obtain a composite material slurry consisting of tuff rock powder waste and coarse aggregate;

[0047] (4) The prepared composite material slurry was poured into a 100×100×100 mm mold twice, and vibrated on a vibration table for 1 to 2 minutes each time. After smoothing, it was covered with plastic wrap and placed in an oven at 80°C. The mold was removed after 24 hours, and the demolded test piece was directly placed in the oven environment for curing for a certain number of days to obtain composite material 2.

[0048] Effect Example

[0049] The compressive strength of the finished composite materials 1 and 2 prepared in the above Examples 1 and 2 is shown in Table 2 below. Figure 2 Schematic diagram of the compressive strength of each composite material (unit: MPa).

[0050] Table 2 Compressive strength

[0051] Experimental subjects 7-day compressive strength 14-day compressive strength 28 days compressive strength Composite Materials 1 26.57 40.07 47.23 Composite Materials 2 31.30 48.90 58.53

[0052] The test results in Table 2 show that in composite material 1, when the tuff stone powder waste component accounts for 11.67% and the blast furnace slag powder accounts for 5.00%, the 7-day, 14-day and 28-day compressive strengths of the tuff stone powder waste and coarse aggregate composite material are 26.57MPa, 40.07MPa and 47.23MPa respectively. The compressive strength at each age is above 25MPa, which can meet the basic actual needs of the project. In contrast, in composite material 2, the tuff stone powder waste component accounts for 10.00% and the blast furnace slag powder accounts for 6.67%. The 7-day, 14-day and 28-day compressive strengths of the composite material are 31.30MPa, 48.90MPa and 58.53MPa respectively. The 7d strength increases by 17.8%, the 14d strength increases by 22.0%, and the 28d strength increases by 23.9%. The compressive strength at each age is improved. At this time, the strength of the composite material at each age is above 30MPa. The above results show that while keeping the mass proportion of powder material in the composite material unchanged, reducing the tuff stone powder waste component and increasing the blast furnace slag powder component can improve the compressive strength of the composite material.

[0053] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A composite material prepared from tuff stone powder waste, characterized in that: The composite material comprises the following components by weight: 10.00-11.67 parts of tuff stone powder waste, 5.00-6.67 parts of blast furnace slag powder, 33.40 parts of sand, 40.8 parts of crushed stone and 9.13 parts of alkali solution.

2. The composite material according to claim 1, characterized in that The tuff stone powder waste is solid waste generated in the process of dry-process sand production, and its specific surface area is between 1100 and 1250 m 2 / kg, the particle size is above 350 mesh, the silicon dioxide content is greater than 40%, and the aluminum oxide content is greater than 12%.

3. The composite material according to claim 1, characterized in that The blast furnace slag powder is S95 grade granulated blast furnace slag powder, and its specific surface area is 700-950m 2 / kg, the particle size is 1-120μm, the calcium oxide content is not less than 33%, and the aluminum oxide content is not higher than 15%.

4. The composite material according to claim 1, characterized in that The sand is selected from one or more of natural sand, river sand and machine-made sand; The crushed stone is selected from one or more of tuff crushed stone, diabase crushed stone, granite crushed stone, basalt crushed stone and recycled construction waste crushed stone.

5. The composite material according to claim 4, characterized in that The sand is machine-made sand made from tuff, with an apparent density of 2.77 g / cm 3 The water absorption rate is 2.06% and the particle size is less than 5mm.

6. The composite material according to claim 1, characterized in that The crushed stone is natural diabase crushed stone with an apparent density of 2300-3800 kg / m 3 The particle size range is 5 to 20 mm, the crushed stone with a particle size of 5 to 10 mm accounts for 20 to 26% of the total mass of the crushed stone, and the crushed stone with a particle size of 10 to 20 mm accounts for 74 to 80% of the total mass of the crushed stone.

7. The composite material according to claim 1, characterized in that The alkali solution is selected from one or more of sodium hydroxide solution, potassium hydroxide solution and sodium silicate solution.

8. The composite material according to claim 7, characterized in that The alkali solution is composed of a sodium hydroxide solution with a volume concentration of 24% and a sodium silicate solution with a volume concentration of 2.0% in a volume ratio of 90.47:9.

53.

9. The method for preparing the composite material according to any one of claims 1 to 8, characterized in that: The method comprises the following steps: (1) mixing tuff stone powder waste and blast furnace slag powder evenly, adding sand and crushed stone and mixing evenly to obtain a dry mix; (2) adding alkali solution to the dry mix and stirring evenly to obtain a mixture; (3) Pour the mixture into a mold, vibrate and compact it, seal the surface with plastic wrap, and place it in an oven at 80°C for 24 hours. De-mold the demoulded test piece and cure it in the oven environment to the set age.