High-flow-state secondary lining concrete and preparation method thereof

By optimizing the formula and preparation method of the second lining concrete, combined with the active spherical silicon-aluminum material and admixture technology, the problems of poor fluidity and insufficient strength of the traditional second lining concrete are solved, and high fluidity and high strength are achieved, which are suitable for tunnel engineering. Reduces construction difficulty and defect rate.

CN118908645APending Publication Date: 2024-11-08CHINA TIESIJU CIVIL ENGINEERING GROUP CO LTD +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410836933.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-26
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Traditional second-lined concrete has poor fluidity, insufficient strength, high construction difficulty, and poor fluidity in concrete preparation of igneous rock aggregate, resulting in low construction strength and high defect rate of second-lined concrete, which is difficult to meet the needs of tunnel projects.

Method used

Adopt high-flow two-lined concrete formula, including cement, fly ash, silica fume, stone powder, machine sand, gravel, admixture and gas induction agent, through active sphere silicon aluminum materials silica fume, fly ash and stone powder compound Doping technology and admixture and gas inducer composite technology optimize material ratio and preparation methods, and improve the flowability, strength and durability of concrete.

Benefits of technology

It achieves high flowability and high strength, reduces construction difficulty and defect rate, improves the working performance and durability of concrete, is suitable for large-scale production and engineering applications, and promotes the production technology of igneous rock powder concrete.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118908645A_ABST
    Figure CN118908645A_ABST
Patent Text Reader

Abstract

The invention discloses high-flow-state secondary lining concrete, which is prepared from the following raw materials in parts by weight: 250 to 400 parts of cement, 20 to 150 parts of fly ash, 5 to 40 parts of silica fume, 20 to 150 parts of stone powder, 650 to 950 parts of machine-made sand, 700 to 1050 parts of gravel, 3.5 to 6.5 parts of additives, 1 to 4 parts of air entraining agents and 150 to 200 parts of water. The invention further discloses a preparation method of the high-flow-state secondary lining concrete. The high-flow-state secondary lining concrete is prepared by using machine-made gravels, machine-made sand and stone powder processed from igneous mother rock, blending fly ash and silica fume and adding an air entraining agent to entrain air. The concrete production efficiency and the concrete pouring effect are improved, the labor intensity and the secondary lining defect rate are reduced, meanwhile, the application range of igneous rock stone powder concrete is expanded, and the igneous rock stone powder concrete production technology is popularized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of civil engineering, and in particular to a high-fluidity secondary lining concrete and a preparation method thereof. Background Art

[0002] With the continuous development of civil engineering technology, the performance requirements for concrete are getting higher and higher. As an important structural material in tunnel engineering, the performance of secondary lining concrete directly affects the safety and durability of the tunnel. However, the traditional preparation method of secondary lining concrete has problems such as poor fluidity, insufficient strength, and great construction difficulty, resulting in low construction strength, high secondary lining defect rate, and unstable strength and durability indicators of the engineering entity. Construction units face the pressure of railway red line inspection and time-consuming and labor-intensive tunnel defect remediation in the middle and late stages of the project. At the same time, with the comprehensive construction of a large number of infrastructure projects in my country, the demand for sand and gravel aggregates is huge, and it is advisable to use local materials from the perspectives of economy and environment. The disposal of abandoned tunnel slag in tunnel engineering is time-consuming and labor-intensive, and it is imperative to use tunnel slag processing to prepare concrete. However, the existing problems are: the igneous rock aggregate has a high needle-like content and poor particle shape, and the prepared concrete has poor fluidity. Therefore, solving the above problems and researching and developing a high-flow secondary lining concrete for tunnel engineering construction has important practical application value. At the same time, it is conducive to expanding the application scope of tunnel slag igneous rock powder concrete and promoting the production technology of igneous rock powder concrete. Summary of the invention

[0003] The purpose of the present invention is to provide a high-flowability secondary lining concrete and a preparation method thereof, so as to solve the technical problems in the prior art that the secondary lining concrete has poor fluidity, insufficient strength, and great construction difficulty, and that the concrete prepared with igneous rock aggregate has poor fluidity.

[0004] To achieve the above object, one embodiment of the present invention provides a high-flow secondary lining concrete, comprising the following raw materials in proportion by weight:

[0005] 250-400 parts of cement, 20-150 parts of fly ash, 5-40 parts of silica fume, 20-150 parts of stone powder, 650-950 parts of machine-made sand, 700-1050 parts of crushed stone, 3.5-6.5 parts of admixtures, 1-4 parts of air-entraining agent, and 150-200 parts of water.

[0006] In one preferred solution of the present invention, the high-flow secondary lining concrete comprises the following raw materials in proportion by weight:

[0007] 260-350 parts of cement, 20-100 parts of fly ash, 10-30 parts of silica fume, 30-120 parts of stone powder, 700-900 parts of machine-made sand, 800-1000 parts of crushed stone, 4-6 parts of admixture, 2-4 parts of air-entraining agent, and 150-180 parts of water.

[0008] In one preferred solution of the present invention, the high-flow secondary lining concrete comprises the following raw materials in proportion by weight:

[0009] 280-320 parts of cement, 30-60 parts of fly ash, 15-25 parts of silica fume, 60-100 parts of stone powder, 750-850 parts of machine-made sand, 850-950 parts of crushed stone, 4-5 parts of admixture, 2-3 parts of air-entraining agent, and 160-170 parts of water.

[0010] In one preferred embodiment of the present invention, the cement is ordinary Portland cement with a strength grade of 42.5 and a specific surface area of ​​300 m 2 / kg-350m 2 / kg, 28-day flexural strength ≥6.5MPa, compressive strength ≥42.5Mpa.

[0011] In one of the preferred solutions of the present invention, the fly ash is Class II fly ash, with a 28-day activity index of ≥70% and a water requirement ratio of ≤105%.

[0012] In one preferred solution of the present invention, the silica fume is densified silica fume, with a 28-day activity index of ≥85%, a SiO2 content of ≥85%, and a specific surface area of ​​18000m 2 / kg-25000m 2 / kg, water requirement ratio ≤125%.

[0013] In one of the preferred solutions of the present invention, the stone powder is processed from igneous rock cave slag, and its 28-day activity index is ≥95%, and its fluidity ratio is ≥100%.

[0014] In one of the preferred solutions of the present invention, the machine-made sand is processed from igneous rock slag, has a fineness modulus of 2.3-3.0, and a moisture content of ≤0.5%.

[0015] One of the preferred solutions of the present invention is that the crushed stone is processed from igneous rock cave slag, with a continuous gradation of particle size of 5mm-20mm, a crushing value ≤10%, a mud content ≤1.0%, a needle-like particle content ≤5%, and a moisture content ≤0.5%.

[0016] One of the preferred solutions of the present invention is that the admixture is a polycarboxylic acid high-performance admixture with an air content of 3.0%-6.0%, a water reduction rate ≥25%, a water bleeding rate ratio ≤20%, a slump loss of ≤40mm in 1 hour, and a compressive strength ratio of ≥140% after 28 days.

[0017] In one of the preferred solutions of the present invention, the air content of the air entraining agent is ≥3%, the water reduction rate is ≥6%, and the 28-day compressive strength ratio is ≥90%.

[0018] In one of the preferred solutions of the present invention, the water is groundwater, the 28-day compressive strength ratio is ≥90%, and the pH value is >6.5.

[0019] Based on the high-flow secondary lining concrete disclosed in the present invention, the present invention also discloses a preparation method of the high-flow secondary lining concrete, comprising the following steps:

[0020] Weigh each raw material according to the ratio;

[0021] The cement, fly ash, silica fume and stone powder are uniformly mixed to obtain a mixed adhesive material;

[0022] uniformly mixing water, admixture and air-entraining agent to obtain a mixed liquid;

[0023] Add crushed stone, mixed adhesive and machine-made sand into a mixer in sequence and mix them, then add the mixed liquid and continue mixing to obtain a high-flow secondary lining concrete.

[0024] In one of the preferred solutions of the present invention, the mixing time of crushed stone, mixed glue and machine-made sand is 1 min-2 min, and the mixing is continued for 1 min-3 min after the mixed liquid is added.

[0025] In one of the preferred solutions of the present invention, the high-flow secondary lining concrete has a strength of 30MPa-60MPa, a slump of 160mm-240mm, and a slump expansion of 500mm-700mm.

[0026] In summary, the beneficial effects of the present invention are:

[0027] 1. The present invention improves the fluidity, strength and durability of concrete by adding igneous rock powder and utilizing the synergistic combination of multiple technologies such as "active spherical silica-alumina material silica fume, fly ash and stone powder composite technology and admixture and air-entraining agent composite technology". At the same time, the prepared high-flowability secondary lining concrete has good working performance, mechanical properties and durability, strong anti-dispersion, high fluidity and high gap permeability, providing a basis for the large-scale application of machine-made sand and gravel and igneous rock powder in engineering.

[0028] 2. The high-flowability secondary lining concrete of the present invention utilizes slag stone powder to replace common auxiliary cementitious materials and ultrafine particles, and adopts the composite technology of admixtures and air entraining agents to greatly improve the fluidity of concrete.

[0029] 3. The present invention uses machine-made crushed stone, machine-made sand, stone powder processed from igneous parent rock, blended with fly ash and silica fume, and prepares high-flow secondary lining concrete by adding air-entraining agent to entrain air. This improves the concrete production efficiency and concrete pouring effect, reduces labor intensity and secondary lining defect rate, and is conducive to expanding the application scope of igneous rock powder concrete and promoting the production technology of igneous rock powder concrete.

[0030] 4. The present invention achieves high fluidity of the secondary lining concrete and improves construction efficiency by optimizing the material ratio.

[0031] 5. The preparation method of the high-flow secondary lining concrete of the present invention is simple, easy to operate, and suitable for large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 The present invention is a flow chart of a preparation method according to an embodiment of the present invention. DETAILED DESCRIPTION

[0033] The invention provides a high-flow secondary lining concrete, comprising the following raw materials in proportion by weight: 250-400 parts of cement, 20-150 parts of fly ash, 5-40 parts of silica fume, 20-150 parts of stone powder, 650-950 parts of machine-made sand, 700-1050 parts of crushed stone, 3.5-6.5 parts of admixture, 1-4 parts of air entraining agent, and 150-200 parts of water;

[0034] Preferably, the high-flow secondary lining concrete comprises the following raw materials in proportion by weight: 260-350 parts of cement, 20-100 parts of fly ash, 10-30 parts of silica fume, 30-120 parts of stone powder, 700-900 parts of machine-made sand, 800-1000 parts of crushed stone, 4-6 parts of admixture, 2-4 parts of air entraining agent, and 150-180 parts of water;

[0035] Preferably, the high-flow secondary lining concrete comprises the following raw materials in proportion by weight: 280-320 parts of cement, 30-60 parts of fly ash, 15-25 parts of silica fume, 60-100 parts of stone powder, 750-850 parts of machine-made sand, 850-950 parts of crushed stone, 4-5 parts of admixture, 2-3 parts of air entraining agent, and 160-170 parts of water;

[0036] Among them, the cement is ordinary Portland cement, with a strength grade of 42.5 and a specific surface area of ​​300m 2 / kg-350m 2 / kg, 28-day flexural strength ≥6.5MPa, compressive strength ≥42.5Mpa; fly ash is Class F II fly ash, spherical particle shape, its 28-day activity index ≥70%, water requirement ratio ≤105%; silica ash is densified silica ash, 28-day activity index ≥85%, SiO2 content ≥85%, specific surface area of ​​18000m 2 / kg-25000m 2 / kg, water requirement ratio ≤125%; stone powder is the part with a particle size of less than 75μm screened out during the process of igneous rock slag being processed into machine-made sand and gravel by jaw crusher, with a 28-day activity index ≥95% and a fluidity ratio ≥100%; machine-made sand is the igneous rock slag being processed by jaw crusher, with a fineness modulus of 2.3-3.0 and a moisture content of ≤0.5%; crushed stone is the nearly round particles processed by igneous rock slag by jaw crusher, with a continuous gradation of particle size of 5mm-20mm, and a crushing value of ≤10%, mud content ≤1.0%, needle-like particle content ≤5%, moisture content ≤0.5%; the admixture is a polycarboxylic acid high-performance admixture with an air content of 3.0%-6.0%, a water reduction rate ≥25%, a water seepage rate ratio ≤20%, a slump loss in 1 hour ≤40mm, and a 28-day compressive strength ratio ≥140%; the air content of the air-entraining agent is ≥3%, a water reduction rate ≥6%, and a 28-day compressive strength ratio ≥90%; the water is groundwater, the 28-day compressive strength ratio ≥90%, and the pH value is >6.5.

[0037] The present invention also discloses a method for preparing a high-fluidity secondary lining concrete, comprising the following steps:

[0038] Weigh the raw materials according to the proportion, including cement, fly ash, silica fume, stone powder, machine-made sand, crushed stone, admixture, air entraining agent and water;

[0039] The weighed cement, fly ash, silica fume and stone powder are uniformly mixed to obtain a mixed adhesive;

[0040] The weighed water, admixture and air-entraining agent are uniformly mixed to obtain a mixed liquid;

[0041] Add crushed stone, mixed adhesive and machine-made sand into a concrete mixer in sequence and stir for 1-2 minutes, then add the mixed liquid and continue stirring for 1-3 minutes to obtain high-flowability second lining concrete. The prepared high-flowability second lining concrete has a strength of 30MPa-60MPa, a slump of 160mm-240mm, and a slump expansion of 500mm-700mm.

[0042] Comparative Example

[0043] The calculation steps and preparation method of the ordinary C35 secondary lining concrete mix ratio include the following steps:

[0044] Step 1: Calculate the trial strength = 35 + 1.645 × 5 = 43.2 MPa;

[0045] Step 2: Calculate the 28-day compressive strength of cementitious materials = 42.5 × 1.16 × 0.70 × 1.00 = 34.5 MPa;

[0046] Step 3: Calculate the concrete water-binder ratio = 0.53 × 34.5 / (43.2 + 0.53 × 0.20 × 34.5) = 0.39. According to experience, the water-binder ratio is 0.38.

[0047] Step 4: Calculate the water consumption per cubic meter of concrete, check the table and determine it is 230kg based on experience, the actual water consumption is 230×(1-0.27)=168kg;

[0048] Step 5: Calculate the amount of cementitious materials per cubic meter of concrete = 168 / 0.38 = 442kg; fly ash amount = 442×35% = 155kg; cement amount = 442-155 = 287kg;

[0049] Step 6: Calculate the amount of admixture per cubic meter of concrete = 442 × 1.0% = 4.42kg, the solid content of the admixture is 24.1%, the water content = 4.42 × (1-24.1%) = 3.35kg, then after deducting the water mass in the admixture, the water content per cubic meter of concrete is 165kg; the amount of air entraining agent = 442 × 0.5% = 2.21kg;

[0050] Step 7: Calculate the amount of sand used per cubic meter of concrete = (2400-165-442) × 45% = 806 kg;

[0051] Step 8: Calculate the amount of crushed stone per cubic meter = 2400-165-442-806 = 987 kg;

[0052] Step 9: Calculate the proportion of concrete materials per cubic meter

[0053] The usage ratio of cement: silica fume: fly ash: stone powder: machine-made sand: crushed stone: admixture: air entraining agent: water is 287: 0: 155: 0: 806: 987: 4.42: 0: 165;

[0054] Step 10: According to step 9, ordinary Portland cement, Class F II fly ash, machine-made sand, machine-made crushed stone with a particle size of (5-20) cm, polycarboxylic acid type high-performance admixture and water are weighed;

[0055] Step 11: Evenly mix the weighed ordinary Portland cement and Class F II fly ash to obtain a mixed adhesive;

[0056] Step 12: Evenly mix the weighed water and the polycarboxylic acid high-performance admixture to obtain a mixed solution;

[0057] Step 13: Put machine-made crushed stone, mixed adhesive and machine-made sand into the concrete mixer in turn, stir for 1-2 minutes, then add the mixed liquid and stir for 1-3 minutes to obtain ordinary secondary lining concrete.

[0058] Among them, the admixture is a polycarboxylic acid high-performance water-reducing agent, specifically hydroxybutyl vinyl polyoxyethylene ether, and the air-entraining agent is an alkylbenzene sulfonate air-entraining agent, specifically sodium dodecylbenzene sulfonate and sodium dodecyl sulfate.

[0059] Example 1

[0060] A high-flowable secondary lining concrete, which is different from the comparative example in that the mixture of 35% fly ash is changed to 5% silica ash + 25% fly ash + 5% stone powder, wherein the stone powder is igneous rock powder. The weight ratio of the high-flowable secondary lining concrete is:

[0061] Cement: silica fume: fly ash: igneous rock powder: machine-made sand: crushed stone: admixture: air entraining agent: water = 287: 22: 111: 22: 806: 987: 4.42: 2.21: 165. Among them, the admixture is a polycarboxylic acid high-performance water reducer, specifically isobutylene alcohol polyoxyethylene ether, and the air entraining agent is an alkylbenzene sulfonate, specifically sodium dodecylbenzene sulfonate.

[0062] Example 2

[0063] A high-flowable secondary lining concrete, which is different from the comparative example in that the mixture of 35% fly ash is changed to 5% silica ash + 20% fly ash + 10% stone powder, wherein the stone powder is igneous rock powder. The weight ratio of the high-flowable secondary lining concrete is:

[0064] Cement: silica fume: fly ash: igneous rock powder: machine-made sand: crushed stone: admixture: air entraining agent: water = 287: 22: 89: 44: 806: 987: 4.42: 2.21: 165. Among them, the admixture is a polycarboxylic acid high-performance water reducer, specifically isopentanol polyoxyethylene ether, and the air entraining agent is an alkylbenzene sulfonate, specifically sodium dodecyl sulfate.

[0065] Example 3

[0066] A high-flowable secondary lining concrete, which is different from the comparative example in that the mixture of 35% fly ash is changed to 5% silica ash + 15% fly ash + 15% stone powder, wherein the stone powder is igneous rock powder. The weight ratio of the high-flowable secondary lining concrete is:

[0067] Cement: silica fume: fly ash: igneous rock powder: machine-made sand: crushed stone: admixture: air entraining agent: water = 287: 22: 66: 66: 806: 987: 4.42: 2.21: 165. Among them, the admixture is a polycarboxylic acid high-performance water reducer, specifically hydroxybutyl vinyl polyoxyethylene ether, and the air entraining agent is an alkylbenzene sulfonate, specifically sodium dodecylbenzene sulfonate.

[0068] Example 4

[0069] A high-flowable secondary lining concrete, which is different from the comparative example in that the mixture of 35% fly ash is changed to 5% silica ash + 10% fly ash + 20% stone powder, wherein the stone powder is igneous rock powder. The weight ratio of the high-flowable secondary lining concrete is:

[0070] Cement: silica fume: fly ash: igneous rock powder: machine-made sand: crushed stone: admixture: air entraining agent: water = 287: 22: 44: 89: 806: 987: 4.42: 2.21: 165. Among them, the admixture is a polycarboxylic acid high-performance water reducer, specifically isobutylene alcohol polyoxyethylene ether, and the air entraining agent is an alkylbenzene sulfonate, specifically sodium dodecyl sulfate.

[0071] Example 5

[0072] A high-flowable secondary lining concrete, which is different from the comparative example in that the mixture of 35% fly ash is changed to 5% silica ash + 5% fly ash + 25% stone powder, wherein the stone powder is igneous rock powder. The weight ratio of the high-flowable secondary lining concrete is:

[0073] Cement: silica fume: fly ash: igneous rock powder: machine-made sand: crushed stone: admixture: air entraining agent: water = 287: 22: 22: 111: 806: 987: 4.42: 2.21: 165. Among them, the admixture is a polycarboxylic acid high-performance water reducer, specifically isopentanol polyoxyethylene ether, and the air entraining agent is an alkylbenzene sulfonate, specifically sodium dodecyl sulfate.

[0074] Comparative Example 1

[0075] A common secondary lining concrete, which is different from Example 1 in that the stone powder is sedimentary rock powder. The weight ratio of the common secondary lining concrete is:

[0076] Cement: silica fume: fly ash: sedimentary rock powder: machine-made sand: crushed stone: admixture: air entraining agent: water = 287: 22: 111: 22: 806: 987: 4.42: 2.21: 165. Among them, the admixture is a polycarboxylic acid high-performance water reducer, specifically isobutylene alcohol polyoxyethylene ether, and the air entraining agent is an alkylbenzene sulfonate, specifically sodium dodecylbenzene sulfonate.

[0077] Comparative Example 2

[0078] A common secondary lining concrete, which is different from Example 2 in that the stone powder is sedimentary rock powder. The weight ratio of the common secondary lining concrete is:

[0079] Cement: silica fume: fly ash: sedimentary rock powder: machine-made sand: crushed stone: admixture: air entraining agent: water = 287: 22: 89: 44: 806: 987: 4.42: 2.21: 165. Among them, the admixture is a polycarboxylic acid high-performance water reducer, specifically isopentanol polyoxyethylene ether, and the air entraining agent is an alkylbenzene sulfonate, specifically sodium dodecyl sulfate.

[0080] Comparative Example 3

[0081] A common secondary lining concrete, which is different from Example 3 in that the stone powder is sedimentary rock powder. The weight ratio of the common secondary lining concrete is:

[0082] Cement: silica fume: fly ash: sedimentary rock powder: machine-made sand: crushed stone: admixture: air entraining agent: water = 287: 22: 66: 66: 806: 987: 4.42: 2.21: 165. Among them, the admixture is a polycarboxylic acid high-performance water reducer, specifically hydroxybutyl vinyl polyoxyethylene ether, and the air entraining agent is an alkylbenzene sulfonate, specifically sodium dodecylbenzene sulfonate.

[0083] Comparative Example 4

[0084] A common secondary lining concrete, which is different from Example 4 in that the stone powder is sedimentary rock powder. The weight ratio of the common secondary lining concrete is:

[0085] Cement: silica fume: fly ash: sedimentary rock powder: machine-made sand: crushed stone: admixture: air entraining agent: water = 287: 22: 44: 89: 806: 987: 4.42: 2.21: 165. Among them, the admixture is a polycarboxylic acid high-performance water reducer, specifically isobutylene alcohol polyoxyethylene ether, and the air entraining agent is an alkylbenzene sulfonate, specifically sodium dodecyl sulfate.

[0086] Comparative Example 5

[0087] A common secondary lining concrete, which is different from Example 5 in that the stone powder is sedimentary rock powder. The weight ratio of the common secondary lining concrete is:

[0088] Cement: silica fume: fly ash: sedimentary rock powder: machine-made sand: crushed stone: admixture: air entraining agent: water = 287: 22: 22: 111: 806: 987: 4.42: 2.21: 165. Among them, the admixture is a polycarboxylic acid high-performance water reducer, specifically isopentanol polyoxyethylene ether, and the air entraining agent is an alkylbenzene sulfonate, specifically sodium dodecyl sulfate.

[0089] Performance Testing

[0090] The concrete prepared in the above comparative example, comparative examples 1-5 and examples 1-5 was subjected to performance tests. The concrete's slump, expansion, air content and 1h slump loss and other properties were tested according to GB / T 50080-2016 "Standard for Test Methods for Performance of Ordinary Concrete Mixtures"; a cubic standard test block with a side length of 150 mm was made according to GB / T 50081-2016 "Standard for Test Methods for Mechanical Properties of Ordinary Concrete", and the compressive strength of the standard test block after curing for 28 days and 90 days was measured; the concrete electric flux was tested according to GB / T50082-2009 "Standard for Test Methods for Long-term Performance and Durability of Ordinary Concrete", and the test results are shown in Table 1:

[0091] Table 1: Test results of comparative examples, comparative examples 1-5 and embodiments 1-5

[0092]

[0093]

[0094] From the above table, it can be seen that in Examples 1-5, the slump of concrete out of the machine is greater than 200mm, the expansion is greater than 550mm, the slump loss in 1h is less than 40mm, and the working performance and mechanical performance data indicators are better than those of the control group, meeting the use requirements of high-flowing secondary lining concrete. Comparative Examples 1-5 use sedimentary rock powder, and the slump and other properties of concrete are lower than those of Examples 1-5. It can be concluded that by mixing igneous rock powder, using silica fume, fly ash and stone powder compounding technology, and admixture and air entraining agent composite technology, high-flowing secondary lining concrete can be obtained according to the method of the present invention. Specifically, the concrete configured by the weight ratio of each component in Example 4 has the best performance and fully meets the requirements for the construction of high-flowing secondary lining concrete.

[0095] Although the specific implementation of the present invention is described in detail in conjunction with the drawings, it should not be understood as limiting the scope of protection of this patent. Within the scope described in the claims, various modifications and variations that can be made by those skilled in the art without creative work still fall within the scope of protection of this patent.

Claims

1. A high-flow secondary lining concrete, characterized in that: The invention comprises the following raw materials in proportion by weight: 250-400 parts of cement, 20-150 parts of fly ash, 5-40 parts of silica fume, 20-150 parts of stone powder, 650-950 parts of machine-made sand, 700-1050 parts of crushed stone, 3.5-6.5 parts of admixtures, 1-4 parts of air-entraining agent, and 150-200 parts of water.

2. A high-flow secondary lining concrete as claimed in claim 1, characterized in that: The high-flow secondary lining concrete comprises the following raw materials in proportion by weight: 260-350 parts of cement, 20-100 parts of fly ash, 10-30 parts of silica fume, 30-120 parts of stone powder, 700-900 parts of machine-made sand, 800-1000 parts of crushed stone, 4-6 parts of admixture, 2-4 parts of air-entraining agent, and 150-180 parts of water.

3. A high-flow secondary lining concrete as claimed in claim 2, characterized in that: The high-flow secondary lining concrete comprises the following raw materials in proportion by weight: 280-320 parts of cement, 30-60 parts of fly ash, 15-25 parts of silica fume, 60-100 parts of stone powder, 750-850 parts of machine-made sand, 850-950 parts of crushed stone, 4-5 parts of admixture, 2-3 parts of air-entraining agent, and 160-170 parts of water.

4. A high-flow secondary lining concrete as claimed in claim 1, 2 or 3, characterized in that: The cement is ordinary Portland cement with a strength grade of 42.5 and a specific surface area of ​​300m 2 / kg-350m 2 / kg, 28-day flexural strength ≥6.5MPa, compressive strength ≥42.5Mpa.

5. A high-flow secondary lining concrete as claimed in claim 1, 2 or 3, characterized in that: The fly ash is Class II fly ash, with a 28-day activity index of ≥70% and a water demand ratio of ≤105%.

6. A high-flow secondary lining concrete as claimed in claim 1, 2 or 3, characterized in that: The silica fume is a densified silica fume with a 28-day activity index of ≥85%, a SiO2 content of ≥85%, and a specific surface area of ​​18,000 m 2 / kg-25000m 2 / kg, water requirement ratio ≤125%.

7. A high-flow secondary lining concrete as claimed in claim 1, 2 or 3, characterized in that: The stone powder is processed from igneous rock cave slag, with a 28-day activity index of ≥95% and a fluidity ratio of ≥100%.

8. A high-flow secondary lining concrete as claimed in claim 1, 2 or 3, characterized in that: The machine-made sand is processed from igneous rock cave slag, has a fineness modulus of 2.3-3.0, and a moisture content of ≤0.5%.

9. A high-flow secondary lining concrete as claimed in claim 1, 2 or 3, characterized in that: The crushed stone is processed from igneous rock cave slag, with a continuous gradation of particle size of 5mm-20mm, a crushing value of ≤10%, a mud content of ≤1.0%, a needle-like particle content of ≤5%, and a moisture content of ≤0.5%.

10. A high-flow secondary lining concrete as claimed in claim 1, 2 or 3, characterized in that: The admixture is a polycarboxylic acid high-performance admixture with an air content of 3.0%-6.0%, a water reduction rate of ≥25%, a water bleeding rate ratio of ≤20%, a slump loss of ≤40mm in 1 hour, and a compressive strength ratio of ≥140% in 28 days.

11. A high-flow secondary lining concrete as claimed in claim 1, 2 or 3, characterized in that: The air content of the air entraining agent is ≥3%, the water reduction rate is ≥6%, and the 28-day compressive strength ratio is ≥90%.

12. A high-flow secondary lining concrete as claimed in claim 1, 2 or 3, characterized in that: The water is groundwater, with a 28-day compressive strength ratio of ≥90% and a pH value of >6.

5.

13. A method for preparing a high-flow secondary lining concrete according to any one of claims 1 to 12, characterized in that: The following steps are involved: Weigh each raw material according to the ratio; The cement, fly ash, silica fume and stone powder are uniformly mixed to obtain a mixed adhesive material; uniformly mixing water, admixture and air-entraining agent to obtain a mixed liquid; Add crushed stone, mixed adhesive and machine-made sand into a mixer in sequence and mix them, then add the mixed liquid and continue mixing to obtain a high-flow secondary lining concrete.

14. A method for preparing a high-flow secondary lining concrete according to claim 13, characterized in that: The mixing time of the crushed stone, mixed glue and machine-made sand is 1 min-2 min, and the mixing is continued for 1 min-3 min after the mixed liquid is added.

15. The method for preparing a high-flow secondary lining concrete according to claim 13, characterized in that: The high-flow secondary lining concrete has a strength of 30MPa-60MPa, a slump of 160mm-240mm, and a slump expansion of 500mm-700mm.