Newly produced steel slag surface modification material, modified steel slag aggregate and application

By combining the modified materials of the surface of the newly produced steel slag, using components such as gelling materials and nanomaterials to form a dense thin shell structure, the problem of large volume expansion of the newly produced steel slag is solved, and the steel slag in building materials is realized. Improved stability and interface performance, suitable for steel slag treatment of all sizes.

CN118908648APending Publication Date: 2024-11-08SHANDONG TRAFFIC PLANNING DESIGN INST
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410953243.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-16
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The high content of free calcium oxide and magnesium oxide in new steel slag results in large volume expansion, which limits the large-scale promotion and application of steel slag in building materials. The existing treatment methods are costly or have high equipment requirements, which are not suitable for all steel plants.

Method used

Using newly produced steel slag surface modified materials, a simple mixing method is designed to form modified steel slag aggregates through the combination of gelling materials, active powder materials, ultra-fine high-active mineral blends and nanomaterials. The active components react with the free components in the steel slag, reduce volume expansion, and form a dense thin shell structure through the emulsion and the hydrophobic components of the nanomaterial, improving the interface performance of the steel slag.

Benefits of technology

It realizes the reduction of the volume expansion and water absorption of steel slag, enhances the crushing value and interface bonding performance of steel slag, simplifies the processing process, does not require long-term placement or special equipment, and is suitable for steel slag sources of various sizes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004947814680000101
    Figure BDA0004947814680000101
  • Figure BDA0004947814680000111
    Figure BDA0004947814680000111
  • Figure BDA0004947814680000112
    Figure BDA0004947814680000112
Patent Text Reader

Abstract

The invention relates to a newly-produced steel slag surface modification material, a modified steel slag aggregate and application, and belongs to the technical field of industrial waste residue recycling. The surface modification material comprises 30-70 parts of a cementing material; 15 to 40 parts of an active powder material; 5-10 parts of a superfine high-activity mineral admixture; 0.02 to 0.5 part of a nano material; 1-4 parts of an emulsion; 1-5 parts of a water reducing agent; 0.1-3 parts of a water reducing agent; the active powder material comprises one or more of fly ash, granulated blast furnace slag and phosphorus slag powder; the superfine high-activity mineral admixture is a submicron mineral admixture and comprises one or more of silica fume, superfine fly ash, superfine steel slag powder and superfine slag powder; the nano material comprises nano silicon dioxide and anatase type nano titanium dioxide. The steel slag aggregate modification method provided by the invention does not need to be placed for a long time and is short in treatment time; no special equipment is needed, and the technological process is simple. The method can be widely applied to steel slag sources of various scales.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of industrial waste slag recycling, and specifically relates to a newly produced steel slag surface modification material, modified steel slag aggregate and application thereof. Background Art

[0002] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention, and should not necessarily be regarded as an admission or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art.

[0003] Steel slag is solid waste discharged during the steelmaking process, and its output is about 12% to 15% of crude steel output. Steel slag has many advantages as aggregate for road materials. The cost of steel slag aggregate is only 10% to 20% of limestone aggregate. If it is used in base materials and surface materials, the comprehensive cost can be reduced by 10% to 30%. The low cost and green environmental protection characteristics make steel slag disposal and the development and utilization of road materials more and more popular. However, affected by the steelmaking process, there are free calcium oxide and magnesium oxide in steel slag. The volume expansion of this kind of free components after contact with water reaches 100% or more. Mixing this kind of steel slag into building materials can easily cause cracking of buildings and structures. In particular, the free component content in the newly produced steel slag is higher and the volume expansion rate is greater. This shortcoming greatly limits the large-scale promotion and application of steel slag.

[0004] To address this issue, current treatment methods for reducing the expansion of steel slag include: aging process, hot slag pouring process, shallow plate slag process, water quenching slag process, air quenching slag process and carbonation process. The aging method is to pile up the newly produced steel slag in the material yard for half a year or even longer to gradually dissolve the free components in the steel slag. This method has a low cost, but the time cycle is too long and the time cost is too high. The hot slag pouring process, shallow plate slag process, water quenching slag process, air quenching slag process and carbonation process require the construction of special equipment, and the technical requirements of the equipment are high, and the initial investment is large, so it is not suitable for all steel mills. Summary of the invention

[0005] In view of the deficiencies in the prior art, the purpose of the present invention is to provide a surface modification material for newly produced steel slag, modified steel slag aggregate and application, and to use the modified material to modify the surface of newly produced steel slag by a simple mixing method, thereby compensating for the deficiencies of steel slag when used as aggregate for pavement materials and expanding the application scenarios of steel slag.

[0006] In order to achieve the above object, the technical solution of the present invention is:

[0007] In the first aspect, a newly produced steel slag surface modification material is prepared using the following components in parts by weight:

[0008] 30-70 parts of cementitious materials; 15-40 parts of active powder materials; 5-10 parts of ultrafine high-activity mineral admixtures; 0.02-0.5 parts of nanomaterials; 1-4 parts of emulsion; 1-5 parts of water reducer; 0.1-3 parts of defoamer; 0.3-0.8 parts of accelerator; 15-20 parts of water;

[0009] The active powder material includes: one or more of fly ash, granulated blast furnace slag and phosphorus slag powder;

[0010] Ultrafine high-activity mineral admixtures are submicron-level mineral admixtures, including: one or more of silica fume, ultrafine fly ash, ultrafine steel slag powder and ultrafine slag powder;

[0011] The nanometer material includes: nanometer silicon dioxide and anatase nanometer titanium dioxide, and the mass ratio of the two is in the range of (2-7): (3-8).

[0012] The emulsion includes one or more of styrene-butadiene emulsion, epoxy resin emulsion and silane emulsion.

[0013] Optionally, the cementitious material is hydraulic, pozzolanic or latently hydraulic;

[0014] Optionally, the cementitious material includes one or more of silicate cement, aluminate cement, sulphoaluminate cement, ferroaluminate cement, fluoroaluminate cement, phosphate cement, supersulfate cement and geopolymer cementitious material.

[0015] Optionally, the nanomaterial further includes: one or more of nano calcium carbonate, nano kaolin, nano montmorillonite, graphene, carbon nanotube and nano alumina.

[0016] Optionally, the water reducer includes one or more of: polycarboxylic acid water reducer, naphthalene water reducer, anthracene water reducer, lignin sulfonate water reducer, humic acid water reducer, aminosulfonate water reducer, aliphatic water reducer, melamine water reducer and coumarone water reducer;

[0017] Optionally, the accelerating setting agent includes one or more of an alumina clinker accelerating setting agent, a water glass accelerating setting agent, an aluminate accelerating setting agent and an aluminum sulfate accelerating setting agent.

[0018] Optionally, 0.1 to 3 parts by mass of a defoaming agent is also added to the newly produced steel slag surface modification material.

[0019] Optionally, the defoaming agent includes: one or more of a polyether defoaming agent, a silicone defoaming agent and a polyether-modified silicone defoaming agent.

[0020] In a second aspect, a method for surface modification of freshly produced steel slag using the above-mentioned freshly produced steel slag surface modification material comprises the following steps:

[0021] S1, slowly premixing the gelling material, the ultrafine mineral admixture and the nanomaterial according to a set ratio to obtain a first mixture;

[0022] S2, keeping the first mixture in a slow stirring state, adding water, a water reducing agent and an emulsion in sequence and stirring evenly to obtain a newly produced steel slag surface modified material;

[0023] S3, keep the surface modification material of the newly produced steel slag in a slow stirring state, slowly add the newly produced steel slag, stir evenly, so that the surface of the newly produced steel slag is covered with the modification material;

[0024] S4, spreading the steel slag obtained in S3 in a single layer, setting a curing time, and obtaining modified steel slag aggregate.

[0025] Optionally, in S1, the stirring rate of the slow stirring premix is ​​100 to 300 r / min, and the time is 30 to 60 s.

[0026] Optionally, in S2, after adding water, water reducing agent and emulsion, slowly stir for 120 to 480 seconds, then quickly stir for 60 to 600 seconds, and then reduce the stirring rate to slow stirring, and the stirring rate of fast stirring is 100 to 600 r / min.

[0027] Optionally, in S3, the newly produced steel slag is added in an amount of 30 to 50 times the mass of the modified material. After the newly produced steel slag is added, slow stirring is continued for 300 to 900 seconds.

[0028] Optionally, in S4, after curing until the modified material develops strength and the modified slags do not stick to each other, they are piled up and stored for future use.

[0029] In a third aspect, modified steel slag aggregate is obtained by the above-mentioned method of surface modification of newly produced steel slag.

[0030] In a fourth aspect, the method for surface modification of the newly produced steel slag and / or the application of modified steel slag aggregate in pavement materials.

[0031] The beneficial effects of the present invention are:

[0032] 1. The newly produced steel slag surface modification material provided by the present invention is designed from the following four aspects: (1) The active components of cementitious materials, active powder materials, ultrafine active powder materials and nanomaterials, such as active SiO2 and other components, are used to react with free components in steel slag to achieve the purpose of reducing the volume expansion of steel slag. (2) The aggregate closest packing theory is used to accurately calculate the dosage of raw materials with different particle sizes to form a tightly embedded structure of nano-level active materials, submicron ultrafine mineral admixtures and micron-level cementitious materials. The dense filling of the steel slag surface is achieved to achieve the purpose of reducing the water absorption rate of the steel slag. (3) The emulsion component in the modified material carries various raw materials to the surface of the steel slag at the initial stage of the modified material, reducing the interface thickness between the steel slag and the modified material, laying the foundation for improving the performance of the modified steel slag. (4) The raw materials of the three particle sizes of nano-level active materials, submicron ultrafine mineral admixtures and micron-level cementitious materials mutually stimulate hydration, further filling the remaining gaps on the surface of the steel slag, and finally forming a dense thin shell structure on the surface of the steel slag. The effect of enhancing the crushing value of modified steel slag is achieved. The cement-based modified external interface is more conducive to bonding with cement paste, asphalt and other binder materials, further improving the interface performance of steel slag. (5) In order to further reduce the water absorption rate of steel slag, the emulsion and nanomaterials used in the modified material contain hydrophobic components, which work together with physical filling and hydration reaction filling to strive to reduce the water absorption rate of steel slag to 0, isolate external moisture from contact with steel slag, and prevent steel slag from swelling when it comes into contact with water.

[0033] 2. The steel slag aggregate modification method provided by the present invention does not need to be placed for a long time, and the processing time is short; it does not need to use special equipment, the process is simple, and it can be widely adapted to steel slag sources of various sizes.

[0034] 3. The modified steel slag aggregate provided by the present invention reduces the optimal asphalt dosage of the steel slag surface material because the modified material is filled on the steel slag surface, while improving the volume stability and stability of the surface material. It includes the following four functions: greatly enhancing the volume stability of steel slag aggregate; enhancing the crushing value of steel slag; reducing the water absorption rate of steel slag; and greatly improving the bonding performance of the bonding interface between steel slag and asphalt, cement paste, etc. DETAILED DESCRIPTION

[0035] It should be noted that the following detailed descriptions are exemplary and are intended to provide further explanation of the present invention. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those commonly understood by those skilled in the art to which the present invention belongs.

[0036] It should be noted that the terms used herein are only for describing specific embodiments and are not intended to limit exemplary embodiments according to the present invention. As used herein, unless the context clearly indicates otherwise, the singular form is also intended to include the plural form. In addition, it should be understood that when the terms "comprising" and / or "including" are used in this specification, it indicates the presence of features, steps, operations, devices, components and / or combinations thereof.

[0037] In the following specific implementation manner, the newly produced steel slag refers to: unaged steel slag, which has been stored for less than 30 days.

[0038] A newly produced steel slag surface modification material is prepared using the following components in parts by weight:

[0039] 30-70 parts of cementitious materials; 15-40 parts of active powder materials; 5-10 parts of ultrafine high-activity mineral admixtures; 0.02-0.5 parts of nanomaterials; 1-4 parts of emulsion; 1-5 parts of water reducer; 0.1-3 parts of defoamer; 0.3-0.8 parts of accelerator and 15-20 parts of water;

[0040] The active powder material includes: one or more of fly ash, granulated blast furnace slag and phosphorus slag powder;

[0041] Ultrafine high-activity mineral admixtures are submicron-level mineral admixtures, including: one or more of silica fume, ultrafine fly ash, ultrafine steel slag powder and ultrafine slag powder;

[0042] The nanometer material includes: nanometer silicon dioxide and anatase nanometer titanium dioxide, and the mass ratio of the two is in the range of (2-7): (3-8).

[0043] The emulsion includes, but is not limited to, one or more of styrene-butadiene emulsion, epoxy resin emulsion and silane emulsion.

[0044] Through the above scheme, the active components react with the free components in the steel slag to achieve the purpose of reducing the volume expansion of the steel slag; the raw materials of different particle sizes are tightly embedded in each other to form a thin shell structure, so as to achieve dense filling of the surface of the steel slag, which not only achieves the purpose of reducing the water absorption rate of the steel slag, but also improves the bonding properties of cement slurry, asphalt and other binder materials; the emulsion component reduces the slurry thickness on the surface of the steel slag to avoid affecting the performance of the steel slag; the emulsion and nanomaterials both contain hydrophobic components, which work together with physical filling and hydration reaction filling to isolate external moisture from contacting the steel slag and prevent the steel slag from swelling when it encounters water.

[0045] The cementitious material has hydraulic properties, volcanic ash activity or potential hydraulic properties; various cements, geopolymers and solid waste-based cementitious materials can be selected; the cementitious material is the main component of the modified material and provides strength for the modified layer;

[0046] The cementitious material includes one or more of silicate cement, aluminate cement, sulphoaluminate cement, ferroaluminate cement, fluoroaluminate cement, phosphate cement, super-sulfate cement and geopolymer cementitious material.

[0047] The role of active powder materials is to increase the proportion of active components in the modified materials and assist the cementitious materials in establishing the mechanical strength of the steel slag thin layer, while reducing the overall cost of the modified materials.

[0048] The principle of adding ultrafine mineral admixtures includes: the particle size of mineral admixtures such as fly ash and slag powder is generally in the micron level, which is basically the same as the particle size of cementitious materials, and the physical filling effect is not obvious; in order to achieve the dense stacking effect of materials with multiple particle sizes, the present invention adds ultrafine mineral admixtures. In addition to playing a structural embedding role, this type of material also participates in the hydration reaction of the cementitious system, further improving the performance of the modified layer.

[0049] The role of nanomaterials is to provide nano-scale material filling and assist the hydration reaction of the gelling system and the physical bonding of the latex. The basic components are nano-silicon dioxide and anatase nano-titanium dioxide. Nano-silicon dioxide has the ability to promote hydration and can quickly form a thin shell structure on the surface of steel slag. Anatase nano-titanium dioxide is hydrophobic and can prevent water on the outside of the thin shell structure from penetrating into the steel slag inside the thin shell structure, thus preventing the steel slag from swelling when it encounters water.

[0050] Nanomaterials that can be added as auxiliary materials include: one or more of nano calcium carbonate, nano kaolin, nano montmorillonite, graphene, carbon nanotubes and nano alumina. The main functions of nanomaterials are: to promote early hydration of modified materials, fill the gaps of hydration products of modified materials, and form a hydrophobic layer.

[0051] Water reducers are mainly used to adjust the rheological properties of cement paste; they include: one or more of polycarboxylic acid water reducers, naphthalene water reducers, anthracene water reducers, lignin sulfonate water reducers, humic acid water reducers, aminosulfonate water reducers, aliphatic water reducers, melamine water reducers and coumarone water reducers.

[0052] The main functions of the accelerator are to promote the hydration reaction of the modified material gelling system, accelerate the establishment of the strength of the modified layer thin shell structure, and shorten the paving time after the modified steel slag is stirred. It includes one or more of alumina clinker accelerators, water glass accelerators, aluminate accelerators and aluminum sulfate accelerators.

[0053] 0.1 to 3 parts by mass of a defoaming agent may also be added to the newly produced steel slag surface modification material.

[0054] The function of the defoaming agent is: a large number of mechanical stirring bubbles will inevitably be generated during the stirring process of the modified material slurry. The addition of the defoaming agent will greatly reduce the number of bubbles in the slurry, ensuring that the slurry will be evenly coated on the surface of the slag to form a dense protective layer; the defoaming agent includes: one or more of polyether defoaming agents, silicone defoaming agents and polyether modified silicone defoaming agents.

[0055] The purpose of adding water is to react with the cementitious material to hydrate the cement and form strength. To determine its dosage, the curve of the change of the water absorption of the steel slag over time should be tested first, and the hydration rate of the cementitious system of the modified material should be combined. Ensure that the amount of water added can still meet the hydration reaction of the modified material after the steel slag absorbs the moisture of the modified material.

[0056] The method for surface modification of freshly produced steel slag using the above-mentioned freshly produced steel slag surface modification material comprises the following steps:

[0057] S1, slowly premixing the gelling material, the ultrafine mineral admixture and the nanomaterial according to a set ratio to obtain a first mixture;

[0058] S2, keeping the first mixture in a slow stirring state, adding water, a water reducing agent and an emulsion in sequence and stirring evenly to obtain a newly produced steel slag surface modified material;

[0059] S3, keep the surface modification material of the newly produced steel slag in a slow stirring state, slowly add the newly produced steel slag, stir evenly, so that the surface of the newly produced steel slag is covered with the modification material;

[0060] S4, spreading the steel slag obtained in S3 in a single layer, curing for a set time, and obtaining modified steel slag aggregate.

[0061] In S1, the stirring rate of the slow stirring premix is ​​100 to 300 r / min, and the time is 30 to 60 s.

[0062] In S2, after adding water, water reducing agent and emulsion, stir slowly for 120 to 480 seconds, then stir rapidly for 60 to 600 seconds, and then reduce the stirring rate to slow stirring, and the stirring rate of rapid stirring is 100 to 600 r / min; the slow stirring rate is the same as the stirring rate of slow stirring premixing in S1.

[0063] In S3, after the addition of the new steel slag is completed, the accelerator is added and the slow stirring is continued for 300 to 900 seconds so that the surface of the new steel slag is covered with the modified material and a thin shell structure is initially formed.

[0064] In S4, after curing until the modified material develops strength and the modified slags do not stick to each other, they are piled up and stored for later use.

[0065] Example 1

[0066] A newly produced steel slag surface modification material is prepared using the following components in parts by weight:

[0067] 50 parts of P·O42.5 ordinary Portland cement, 20 parts of Class I fly ash materials, 8 parts of silica fume, 0.2 parts of nano silicon dioxide, 0.2 parts of nano titanium dioxide, 2.6 parts of polycarboxylic acid water reducer, 0.5 parts of alkali-free accelerator and 2.0 parts of styrene-butadiene emulsion, 0.5 parts of polyether defoamer and 16 parts of water.

[0068] The preparation method comprises:

[0069] First, the gelling material, active powder material, ultrafine powder material, nano-silicon dioxide and nano-titanium dioxide were premixed slowly for 60 seconds at a stirring rate of 200 r / min;

[0070] Add mixing water, polycarboxylate water reducer and styrene-butadiene emulsion to the premix in sequence under slow stirring, and continue to stir slowly for 180 seconds; then stir rapidly for 180 seconds at a stirring speed of 600 r / min, and then reduce the stirring speed to slow;

[0071] Slowly pour 4000 parts by weight of steel slag into the stirred slurry under slow stirring, then add alkali-free accelerating agent, and continue stirring for 300 seconds until the aggregate particles are distinct;

[0072] Finally, the steel slag coated with the modified material is spread evenly, and the single layer of steel slag should not overlap. After the modified material forms strength and the steel slag does not stick to each other, it can be piled up for use.

[0073] Example 2

[0074] A newly produced steel slag surface modification material is prepared using the following components in parts by weight:

[0075] 30 parts of P·O42.5 ordinary Portland cement, 15 parts of Class I fly ash materials, 5 parts of silica fume, 0.01 parts of nano silicon dioxide, 0.01 parts of nano titanium dioxide, 5 parts of polycarboxylic acid water reducer, 0.3 parts of alkali-free accelerator, 0.1 parts of polyether defoamer, 1 part of styrene-butadiene emulsion and 15 parts of water.

[0076] The preparation method is the same as that in Example 1.

[0077] Example 3

[0078] A newly produced steel slag surface modification material is prepared using the following components in parts by weight:

[0079] 70 parts of PO42.5 ordinary Portland cement, 40 parts of Class I fly ash material, 10 parts of silica fume, 0.25 parts of nano silicon dioxide, 0.25 parts of nano titanium dioxide, 5 parts of polycarboxylic acid water reducer, 0.8 parts of alkali-free quick setting agent, 3 parts of polyether defoamer, 4 parts of styrene-butadiene emulsion and 20 parts of water. The preparation method is the same as that of Example 1.

[0080] Comparative Example 1

[0081] The steel slag from the same source as in Example 1 was dried and loaded into a mixer, the mixer was started, and a water repellent was sprayed into the mixing pot with a spray bottle until the surface of the steel slag was completely wetted; the water repellent was a nano-silicon water repellent, and the mass ratio of the added mass of the water repellent to the mass of the steel slag was 1:300.

[0082] The steel slag is poured out and dried for later use, thereby obtaining the modified steel slag aggregate of this comparative example.

[0083] Comparative Example 2

[0084] Weigh 4 parts of P·O 42.5 ordinary Portland cement, pour in 0.16 parts of mixing water under slow stirring, and stir slowly for 180 seconds at a stirring rate of 200r / min. Then stir quickly for 180 seconds at a stirring rate of 600r / min. Then reduce the stirring rate to slow, and slowly pour 100 parts of steel slag from the same source as in Example 1 into the stirred slurry under slow stirring, and continue stirring for 300s. Finally, spread the cement-wrapped steel slag evenly, requiring that there should be no overlap in the single layer of steel slag, until the cement forms strength and the steel slags do not stick to each other, and then pile them up for use to obtain the modified steel slag aggregate of this comparative example.

[0085] Comparative Example 3

[0086] The steel slag from the same source as that in Example 1 was not processed and was used as the steel slag aggregate of Comparative Example 3.

[0087] Example 4

[0088] Specimen preparation:

[0089] The raw materials were weighed according to the mix ratio shown in Table 1, and the modified steel slag aggregates obtained in Examples 1 to 3 and Comparative Examples 1 to 2 were used to prepare the steel slag base material immersion expansion test pieces; the raw materials were weighed according to the mix ratio shown in Table 2, and the modified steel slag aggregates obtained in Examples 1 to 3 and Comparative Examples 1 to 2 were used to prepare the Marshall test pieces of steel slag asphalt mixtures, and the preparation method adopted the industry standard. In Tables 1 and 2, "steel slag" is the abbreviation of modified steel slag aggregate or steel slag aggregate.

[0090] Table 1

[0091]

[0092] Table 2

[0093]

[0094] Test content:

[0095] Use a cutting machine to vertically cut the asphalt mixture specimen, clean the powder on the cut surface, take photos and record them, and determine whether a thin shell structure is formed based on the structural layer.

[0096] JTG E42-2005 "Highway Engineering Aggregate Test Procedure" tests the crushing value and water absorption rate of steel slag after different surface modification methods;

[0097] GB / T 24175-2009 "Test method for stability of steel slag" tests the water expansion of base materials prepared by steel slag treated with different surface modification methods;

[0098] JTG E51-2009 "Testing Procedures for Stabilized Materials with Inorganic Binders for Highway Engineering" tests the 7-day unconfined compressive strength of base materials prepared from steel slag after different surface modification methods;

[0099] JTG 3432-2024 "Highway Engineering Aggregate Test Procedure" tests the water expansion of surface materials made of steel slag after different surface modification methods;

[0100] JTG E20-2011 "Test Procedures for Asphalt and Asphalt Mixtures in Highway Engineering" tests the stability of surface materials prepared from steel slag after different surface modification methods;

[0101] Test results:

[0102] There is a thin shell-like structural layer between the steel slag aggregate and the green mixture matrix in the asphalt mixture specimens of Examples 1 to 3.

[0103] The JTG E42-2005 performance test results of steel slag aggregate are shown in Table 3.

[0104] Table 3

[0105]

[0106]

[0107] The performance test results of GB / T 24175-2009 and JTG E51-2009 of steel slag base materials are shown in Table 4.

[0108] Table 4

[0109] Test items Cumulative volume expansion rate (%) 7d unconfined strength (MPa) Example 1 (Steel slag of the present invention) 0.45 8.02 Example 2 (Steel slag of the present invention) 0.49 8.26 Example 3 (Steel slag of the present invention) 0.63 7.33 Comparative Example 1 1.72 6.86 Comparative Example 2 2.03 7.42 Comparative Example 3 (untreated steel slag) 2.31 7.27

[0110] The JTG E42-2005 performance test results of the steel slag surface material are shown in Table 5.

[0111] Table 5

[0112] Test items Optimal asphalt dosage (%) Cumulative volume expansion rate (%) Stability (kN) Example 1 (Steel slag of the present invention) 4.5 0.53 10.62 Example 2 (Steel slag of the present invention) 4.6 0.66 10.35 Example 3 (Steel slag of the present invention) 4.5 0.61 10.38 Comparative Example 1 4.5 0.81 10.13 Comparative Example 2 4.8 1.02 10.21 Comparative Example 3 (untreated steel slag) 4.8 0.99 9.83

[0113] It can be seen from the test results that the crushing value and water absorption rate of the steel slag treated with the modified materials of the present invention (Examples 1 to 3) are lower than those of other treatment methods, and meet the relevant standards and can be applied to pavement materials. The treated steel slag was used to prepare the steel slag base material. After testing, the cumulative volume expansion rate of the base material was greatly reduced, proving that the modified materials within the proportion range of the present invention have excellent effects on improving the volume stability of steel slag. The treated steel slag was used to prepare the steel slag surface material. After testing, since the modified material was filled on the surface of the steel slag, the optimal asphalt dosage of the steel slag surface material was reduced, and the volume stability and stability of the surface material were improved. The examples prove that the modified material of the present invention has the functions of greatly enhancing the volume stability of steel slag aggregate, enhancing the crushing value of steel slag, reducing the water absorption rate of steel slag, and greatly improving the bonding performance of the bonding interface between steel slag and asphalt, cement slurry, etc.

[0114] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A new type of steel slag surface modification material, It is characterized in that The following components were used to prepare the product: 30-70 parts of cementitious materials; 15-40 parts of active powder materials; 5-10 parts of ultrafine high-activity mineral admixtures; 0.02-0.5 parts of nanomaterials; 1-4 parts of emulsions; 1-5 parts of water reducing agents; 0.1-3 parts of defoamer; 0.3-0.8 parts of accelerator and 15-20 parts of water; The active powder material includes: one or more of fly ash, granulated blast furnace slag and phosphorus slag powder; Ultrafine high-activity mineral admixtures are submicron-level mineral admixtures, including: one or more of silica fume, ultrafine fly ash, ultrafine steel slag powder and ultrafine slag powder; The nanomaterials include: nano silicon dioxide and anatase nano titanium dioxide, and the mass ratio of the two is in the range of: (2-7): (3-8); The emulsion includes one or more of styrene-butadiene emulsion, epoxy resin emulsion and silane emulsion.

2. The surface modified material of newly produced steel slag according to claim 1, It is characterized in that Cementitious materials are hydraulic, pozzolanic or latently hydraulic; Optionally, the cementitious material includes one or more of silicate cement, aluminate cement, sulphoaluminate cement, ferroaluminate cement, fluoroaluminate cement, phosphate cement, supersulfate cement and geopolymer cementitious material.

3. The surface modified material of newly produced steel slag according to claim 1, It is characterized in that Water reducing agents include: One or more of polycarboxylic acid water reducer, naphthalene water reducer, anthracene water reducer, lignin sulfonate water reducer, humic acid water reducer, aminosulfonate water reducer, aliphatic water reducer, melamine water reducer and coumarone water reducer.

4. The surface modified material of newly produced steel slag according to claim 1, It is characterized in that The accelerating setting agent includes: one or more of alumina clinker accelerating setting agent, water glass accelerating setting agent, aluminate accelerating setting agent and aluminum sulfate accelerating setting agent.

5. The surface modified material of newly produced steel slag according to claim 1, It is characterized in that 0.1 to 3 parts by mass of defoaming agent is added to the surface modification material of the newly produced steel slag; Optionally, the defoaming agent includes: one or more of a polyether defoaming agent, a silicone defoaming agent and a polyether-modified silicone defoaming agent.

6. A method for surface modification of freshly produced steel slag using the freshly produced steel slag surface modification material according to any one of claims 1 to 5, It is characterized in that The following steps are involved: S1, slowly premixing the gelling material, the ultrafine mineral admixture and the nanomaterial according to a set ratio to obtain a first mixture; S2, keeping the first mixture in a slow stirring state, adding water, a water reducing agent and an emulsion in sequence and stirring evenly to obtain a newly produced steel slag surface modified material; S3, keep the surface modification material of the newly produced steel slag in a slow stirring state, slowly add the newly produced steel slag, stir evenly, so that the surface of the newly produced steel slag is covered with the modification material; S4, spreading the steel slag obtained in S3 in a single layer, curing for a set time, and obtaining modified steel slag aggregate.

7. The method for surface modification of freshly produced steel slag according to claim 6, It is characterized in that In S1, the stirring rate of the slow premix is ​​100-300 r / min, and the time is 30-60 s; Optionally, in S2, after adding water, water reducing agent and emulsion, slowly stir for 120 to 480 seconds, then quickly stir for 60 to 600 seconds, and then reduce the stirring rate to slow stirring, and the stirring rate of fast stirring is 100 to 600 r / min.

8. The method for surface modification of freshly produced steel slag according to claim 6, It is characterized in that In S3, the amount of newly produced steel slag added is 30 to 50 times the mass of the modified material. After the newly produced steel slag is added, continue to stir slowly for 300 to 900 seconds; Optionally, in S4, after curing until the modified material develops strength and the modified slags do not stick to each other, they are piled up and stored for future use.

9. A modified steel slag aggregate prepared by the method for surface modification of freshly produced steel slag as described in any one of claims 6 to 8.

10. A method for surface modification of newly produced steel slag as claimed in any one of claims 6 to 8 and / or use of modified steel slag aggregate as claimed in claim 9 in pavement materials.