Environment-friendly anti-freezing anti-cracking recycled concrete and preparation method thereof

By using composite coarse aggregate, rock sand, scallop shell powder and multi-fiber structure in recycled concrete, the problem of insufficient anti-freeze and cracking performance of existing recycled concrete is solved, and low-cost and high-performance environmentally friendly regeneration is achieved Concrete preparation.

CN118908650APending Publication Date: 2024-11-08INST OF MOUNTAIN HAZARDS & ENVIRONMENT CHINESE ACADEMY OF SCI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410958615.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing recycled concrete has shortcomings in its frost resistance and crack resistance, and the raw materials are complex, the process costs are high, and it does not have crack resistance.

Method used

Using composite coarse aggregate, specific rock-specific sand and scallop shell powder as blends, combining multi-composite reinforced fiber structures with hemp fiber and plastic fibers, improves the bonding performance and ease of recycled concrete at low cost, and uses low-cost Conventional admixtures simplify the process.

Benefits of technology

It significantly improves the freezing durability and crack resistance of concrete, reduces raw material and process costs, and realizes the preparation of environmentally friendly high-performance recycled concrete.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118908650A_ABST
    Figure CN118908650A_ABST
Patent Text Reader

Abstract

The invention discloses environment-friendly anti-freezing anti-cracking recycled concrete and a preparation method thereof. Aiming at the defects that the raw material and process cost of the existing recycled concrete is relatively high and the existing recycled concrete does not have anti-cracking performance, the invention provides the recycled concrete which comprises the following components: 150-180 parts of water, 370-420 parts of a cementing material, 610-640 parts of coarse aggregate, 520-550 parts of fine aggregate, 40-70 parts of an admixture, 55-60 parts of a reinforcing material and 13-17 parts of an additive, wherein the coarse aggregate comprises broken stone and recycled coarse aggregate, the fine aggregate is rock machine-made sand, the admixture is scallop shell powder, the reinforcing material comprises bast fiber and plastic fiber, and the plastic fiber comprises short fiber and long fiber. According to the concrete disclosed by the invention, various domestic wastes are used as raw materials, only one conventional additive is used, the process is simple, the energy consumption is low, and meanwhile, the concrete has high performance of freezing resistance and cracking resistance, and is environment-friendly concrete in a real sense.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a recycled concrete, in particular to a concrete with high performance of antifreeze and anti-cracking using a variety of waste and recycled materials as raw materials, and a preparation method thereof, belonging to the technical field of recycled concrete and the technical field of waste recycling. Background Art

[0002] With the transition from a production-oriented society to a consumption-oriented society, the use of various materials in human production and life has fallen into a similar two-end expansion mode. In the material use chain, the beginning is the ever-expanding intake of raw materials, and the end is the ever-accumulating waste discharge outlet. The expansion at both ends has jointly formed endless filling pressure and disposal pressure on production and life. Using various types of material recycling and regeneration technologies, building a waste recycling system, and achieving connectivity at both ends is an effective way to simultaneously resolve the pressure at both ends. In the circulation of social production materials, the construction industry occupies both a super-large-scale intake of raw materials and a super-large-scale waste discharge outlet, which has always been a problem for sustainable development.

[0003] Theoretically, construction waste contains a large amount of waste concrete blocks, which are consistent with the components of concrete aggregates. If they are directly processed into commercial concrete aggregates, they can, to a certain extent, constitute the connection, circulation and balance between the consumption of raw materials and the generation of waste in the construction industry. Recycled concrete is such a technology. Recycled concrete is concrete mixed with recycled aggregates, which can be referred to as recycled concrete. Recycled aggregate refers to concrete aggregate made by mechanical crushing and screening of concrete, mortar, and stone in construction / construction waste. With the specialization of people's requirements for the use and performance of concrete, the demand for special / high-performance concrete continues to grow. Therefore, special / high-performance recycled concrete technology is an effective and powerful component of the construction of a waste recycling system.

[0004] Prior art CN 2022115353778 discloses a recycled concrete, which is a high-strength concrete made of recycled aggregates from construction waste mixed with steel slag. The raw materials include reinforced recycled aggregates from construction waste, cement, blast furnace slag powder, silica fume, 35% water glass solution, coarse steel slag aggregate, fine steel slag aggregate, water reducer, polymer cement-based reinforcing material, and water. The performance indicators of this concrete are high strength, impermeability, and excellent frost resistance, and the appearance quality does not frost or crack. The technical defects of this concrete are mainly: 1. The raw materials are complex; 2. The proportion of construction waste aggregates added is low, and it needs to be processed by strengthening technology; 3. The performance does not include crack resistance, but is limited to "the appearance quality does not crack". Prior art CN 2021109892201 discloses a sponge city high-strength recycled aggregate concrete, the raw materials include reinforced recycled coarse aggregate, cement, water, steel slag powder, limestone powder, nano-silicon dioxide, graphene oxide powder, polyacrylate, water glass, water reducer, super absorbent resin, modified reinforcing agent, with stable and lasting compressive strength, wear resistance, frost resistance and deformation resistance. The proportion of construction waste aggregate in this concrete is relatively high, and the technical defects are mainly: 1. The raw materials are diverse, and there are more prefabrication processes, and more admixtures are used, which makes the concrete reaction process complicated, so the raw material and process costs increase; 2. The concrete also does not have anti-cracking performance. Summary of the invention

[0005] The purpose of the present invention is to address the deficiencies of the prior art and to provide an environmentally friendly recycled concrete and a preparation method thereof based on the concept of waste recycling technology.

[0006] To achieve the above-mentioned purpose, the present invention first provides an environmentally friendly frost-resistant and crack-resistant recycled concrete, and its technical solution is as follows.

[0007] The invention discloses an environment-friendly frost-resistant and crack-resistant recycled concrete, the components of which include water, a binder, a coarse aggregate, a fine aggregate, an admixture, a reinforcing material, and an admixture, wherein the binder is cement, and the admixture is a water reducer. The invention is characterized in that the coarse aggregate includes crushed stone and recycled coarse aggregate, the fine aggregate is rock machine-made sand, the admixture is scallop shell powder, the reinforcing material includes hemp fiber and plastic fiber, and the plastic fiber includes plastic short fiber and plastic long fiber; the dosage of each component is 150-180 parts of water, 370-420 parts of a binder, 610-640 parts of a coarse aggregate, 520-550 parts of a fine aggregate, 40-70 parts of an admixture, 55-60 parts of a reinforcing material, and 13-17 parts of an admixture.

[0008] The above-mentioned environmentally friendly frost-resistant and crack-resistant recycled concrete is made by mixing recycled coarse aggregate. By adopting a composite coarse aggregate composed of crushed stone and recycled coarse aggregate, using rock machine-made sand as fine aggregate, and using scallop shell powder to promote cement hydration reaction, the structural defects of recycled aggregate are overcome, and the frost-resistant and durable skeleton structure of recycled concrete is formed together. Among them, the small-particle scallop shell powder can provide excess nucleation sites for the hydrated calcium silicate gel in the hydration reaction product. A large amount of hydrated calcium silicate gel can be filled in the micro-cracks and pores of the concrete matrix together with the scallop shell powder, thereby preventing the invasion of external water back during the freeze-thaw cycle, slowing down the frost heave of water, and significantly improving the frost resistance and durability of concrete. The reinforcing material adopts composite fiber, specifically a composite of various materials and various specifications. Based on the tensile properties of hemp and plastic materials, the former is designed as one specification, and the latter is designed as long and short specifications. According to the previous test data, on the one hand, the use of a single specification for hemp fiber helps to give full play to the toughness characteristics of hemp fiber materials, using the longer hemp fibers to provide restraint for micro cracks in a large spatial range at the micro level, effectively transmitting and dispersing the destructive stress generated by the concrete matrix in a freeze-thaw environment; on the other hand, the use of two specifications of long and short plastic fibers helps to disperse the higher-strength plastic fibers to the maximum extent in the large and small spatial ranges of the concrete matrix, improving the spatial density of concrete at the micro level, thereby effectively limiting the damage evolution process of concrete in a freeze-thaw environment. On this basis, the multi-composite structural design of reinforcing fibers using materials and specifications can give full play to the multi-level and multi-space bridging effect, and be scattered in the concrete matrix and overlapped on the micro cracks, thereby effectively preventing the expansion of cracks during the freeze-thaw cycle, and playing a role in significantly improving the splitting tensile performance of concrete structures in severe cold regions.

[0009] Based on the above-mentioned environmentally friendly frost-resistant and crack-resistant recycled concrete, the present invention further provides an optimized technical solution.

[0010] Optimization 1. Optimization of coarse aggregate: The ratio of crushed stone to recycled coarse aggregate is 1:1, the particle size of crushed stone is 5mm-15mm, and the particle size of recycled coarse aggregate is 10mm-20mm.

[0011] Optimization 2. Optimization of reinforcing materials. The reinforcing materials include 10-40 parts of hemp fiber, 20-50 parts of plastic fiber, and the ratio of plastic short fiber to plastic long fiber is 2:1.

[0012] Optimization 3. Optimization of fine aggregate. Rock machine-made sand is gneiss machine-made sand.

[0013] Optimization 4. Optimization of admixtures. Scallop shell powder is kitchen waste scallop shell powder.

[0014] Optimization 5. Optimization of hemp fiber Hemp fiber is ramie fiber.

[0015] Optimization 6. Optimization of plastic fibers. Plastic fibers are made from discarded plastic straws.

[0016] The present invention also provides a method for preparing the above-mentioned environmentally friendly frost-resistant and crack-resistant recycled concrete, and the specific technical scheme is as follows.

[0017] A method for preparing environmentally friendly frost-resistant and crack-resistant recycled concrete, characterized by:

[0018] First, prepare water, cementing materials, coarse aggregate, fine aggregate, admixtures, reinforcing materials, and admixtures according to the quantity and specifications, including:

[0019] Scallop shell powder: kitchen waste scallop shells are cleaned and disinfected, dried in an oven at 110℃~120℃, and ground into powder; hemp fiber: hemp plants are treated with alkali and dried to make refined hemp fiber, which is processed into fiber; plastic fiber: discarded straws are cleaned and disinfected, crushed and sheared into plastic short fibers and plastic long fibers, and mixed evenly to obtain plastic fibers;

[0020] Then mix the component raw materials according to the following steps:

[0021] Step S100, mixing the admixture and the binder, dispersing by microwave and stirring evenly, to obtain a modified cement-based material;

[0022] Step S200, putting the modified cement-based material, admixture and 1 / 3 of the water into a No. 1 mixer, stirring evenly to obtain a primary mixture;

[0023] Step S300, continue to add coarse aggregate and fine aggregate, stir evenly, and obtain a secondary mixture; add hemp fiber and plastic fiber into the No. 2 mixer, stir evenly, and obtain a reinforcement material;

[0024] Step S400, put the reinforcing material into mixer No. 1, add 1 / 3 of the amount of water, stir evenly, then add 1 / 3 of the amount of water, stir evenly, and obtain a concrete mixture.

[0025] Compared with the prior art, the present invention has the following beneficial effects: (1) Limited by the structural defects of recycled aggregates, in order to obtain special performance of recycled concrete, the prior art generally adopts two means, one is to use a variety of admixtures, and the other is to first modify the recycled aggregate to change its particle structure, especially the surface structure, so as to enhance its "skeleton" function. The recycled concrete of the present invention is different from this. By using three technical means, namely, using composite coarse aggregate, selecting specific rock machine-made sand, and using scallop shell powder as an admixture, the combination performance of recycled coarse aggregate and other skeleton particles is improved in a low-cost manner, thereby improving the workability of recycled concrete mixture. (2) The present invention designs a multi-composite reinforcing fiber composed of hemp fiber and plastic fiber. In particular, considering that when recycled plastic is used as raw material after simple cleaning and disinfection, the recycled plastic fiber has the defects of being brittle and easy to break compared with the original plastic fiber, the present invention provides a single-specification natural hemp fiber mixed with a double-specification recycled plastic fiber to form a reinforcing fiber structure under a multi-level and multi-space bridging effect, thereby overcoming the defects of recycled plastic fiber when used as a reinforcing fiber for antifreeze and anti-cracking recycled concrete in a low-cost manner. (3) The recycled concrete of the present invention uses a variety of domestic waste as raw materials and only uses one conventional admixture. It has a simple preparation process and low energy consumption. It also has high performance in terms of anti-freezing and anti-cracking. It is a truly environmentally friendly concrete. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 It is a schematic diagram of the preparation process of environmentally friendly frost-resistant and crack-resistant recycled concrete.

[0027] FIG. 2 is a schematic diagram showing a comparison of concrete preparation methods. DETAILED DESCRIPTION

[0028] The preferred technical scheme of the present invention is further described below in conjunction with embodiments.

[0029] Embodiment 1

[0030] The environmentally friendly frost-resistant and crack-resistant recycled concrete of the present invention is prepared.

[0031] 1. Preparation of concrete components

[0032] Prepare concrete components according to specifications, including water, cementitious materials, coarse aggregate, fine aggregate, admixtures, reinforcing materials, and admixtures. See Table 1.

[0033] Recycled coarse aggregate: coarse aggregate made from concrete, mortar and stone from construction waste through mechanical crushing and screening.

[0034] Processing of scallop shell powder for admixture: Wash and disinfect kitchen waste scallop shells, bake and dry in an oven at 110℃ ~ 120℃, and grind into powder according to specifications.

[0035] Processing of hemp fiber for reinforcement: Hemp plants are treated with alkali and dried to make refined hemp fiber, which is then processed into fiber according to specifications.

[0036] Plastic fiber for reinforcement: discarded plastic straws are cleaned and disinfected, crushed and sheared, processed into plastic short fibers and plastic long fibers according to specifications, and then mixed evenly to obtain plastic fibers.

[0037] Table 1 List of concrete components

[0038]

[0039] The amounts of each component of concrete are shown in Table 2.

[0040] 2. Preparation of concrete mixture

[0041] Figure 1 It is a schematic diagram of the preparation process of environmentally friendly frost-resistant and crack-resistant recycled concrete.

[0042] Step S100, the admixture and the binder are mixed, dispersed by microwave and stirred evenly (5min to 8min), so as to obtain a modified cement-based material.

[0043] Step S200, putting the modified cement-based material, admixture and 1 / 3 of the water into a No. 1 mixer, stirring evenly (6 min to 9 min) to obtain a primary mixture;

[0044] Step S300, add coarse aggregate and fine aggregate into mixer No. 1, stir evenly (3min-4min), and obtain a secondary mixture; at the same time, add hemp fiber and plastic fiber into mixer No. 2, stir evenly (10min-15min), and obtain a reinforcement material;

[0045] Step S400, put the reinforcing material into mixer No. 1, add 1 / 3 of the amount of water, stir evenly (10min to 13min), then add 1 / 3 of the amount of water, stir evenly (10min to 13min), and obtain a concrete mixture.

[0046] 3. Concrete performance testing

[0047] The concrete mixture is placed in a mold for curing to obtain the environmentally friendly antifreeze and anti-cracking recycled concrete of the present invention, and its performance is tested.

[0048] Split tensile strength: Standard test blocks were made according to GB / T50081-2002 “Standard for test methods of mechanical properties of ordinary concrete”, and the splitting tensile strength of the standard test blocks was measured after 7d and 28d of curing.

[0049] Anti-freeze performance test: refer to GB / T50082 2009 "Standard for test methods of long-term performance and durability of ordinary concrete" to make cubic test blocks and cure for 28 days. Use the quick freezing method to test, and evaluate the anti-freeze performance through the compressive strength and splitting tensile strength of the test blocks under different freeze-thaw cycles.

[0050] The test results are shown in Table 3.

[0051] Embodiment 2

[0052] The environmentally friendly frost-resistant and crack-resistant recycled concrete of the present invention is prepared, and the same points as those in Example 1 are not repeated here, except for the amount of concrete components.

[0053] The amounts of concrete components are shown in Table 2, and the concrete performance test results are shown in Table 3.

[0054] Embodiment 3

[0055] The environmentally friendly frost-resistant and crack-resistant recycled concrete of the present invention is prepared, and the same points as those in Example 1 are not repeated here, except for the amount of concrete components.

[0056] The amounts of concrete components are shown in Table 2, and the concrete performance test results are shown in Table 3.

[0057] Embodiment 4

[0058] The environmentally friendly frost-resistant and crack-resistant recycled concrete of the present invention is prepared, and the same points as those in Example 1 are not repeated here, except for the amount of concrete components.

[0059] The amounts of concrete components are shown in Table 2, and the concrete performance test results are shown in Table 3.

[0060] Table 2 List of dosages of concrete components in Example 1 to Example 4 (unit: part)

[0061]

[0062]

[0063] Table 3 Concrete performance test results of Example 1 to Example 4 (unit: MPa)

[0064]

[0065] Comparing the test results in Table 3 with the prior art, it is shown that: (1) The compressive strength of the concrete of the present invention (taking Example 3 as an example) after 100 freeze-thaw cycles is still as high as 52.8 MPa, and after 300 freeze-thaw cycles, it is only reduced by 10.04% (from 52.8 to 47.5 MPa) compared with 100 freeze-thaw cycles, which is significantly higher than the frost resistance of the existing frost-resistant concrete (reference ZL202010648014X a frost-resistant concrete and its preparation method), and the frost resistance performance is excellent. (2) The splitting tensile strength of the concrete of the present invention (taking Example 3 as an example) is as high as 6.4 MPa when there is no freeze-thaw, and it is still as high as 5.8 MPa after 100 freeze-thaw cycles, which is significantly higher than the crack resistance of the existing anti-cracking concrete (reference ZL2022113367028 a concrete modifier and its preparation method and concrete), and the crack resistance performance is excellent. (3) The concrete prepared in Example 3 has the best splitting tensile strength and frost resistance after curing for 7 days and 28 days.

[0066] Comparative Example 1

[0067] Admixture comparison test 1, removing admixture.

[0068] A concrete is prepared, and the same parts as those in Example 1 are not described in detail. The difference is that the admixture is removed, which is not conducive to the modification of the silicate cement by the kitchen waste scallop shell powder. The corresponding operation steps are omitted in the preparation method.

[0069] The concrete performance test results are shown in Table 4. The test data show that the degree of cement hydration reaction of the concrete specimens has decreased, resulting in the splitting tensile strength and compressive strength data after different freeze-thaw cycles being lower than those in Example 1.

[0070] Comparative Example 2

[0071] Admixture comparison test 2, factory scallops replacing kitchen waste scallops.

[0072] A concrete is prepared, and the same parts as those in Example 1 are not repeated here. The difference is that in the admixture, the kitchen waste scallop shell powder is replaced with factory scallop shell powder of the same specification and mass fraction. The factory scallop shell powder is made from factory scallop waste and is prepared by the same processing method as the kitchen waste scallop shell powder in Example 1.

[0073] The concrete performance test results are shown in Table 4. The test data show that in the concrete of the present invention, the use of kitchen waste scallop shell powder as an admixture is better than the use of factory scallop shell powder as an admixture.

[0074] Table 4 Concrete admixture comparative test performance test results (unit: MPa)

[0075]

[0076] Comparative Example 3

[0077] Reinforcement material comparison test 1, removing ramie fiber.

[0078] A concrete is prepared, and the same parts as those in Example 1 are not described in detail. The difference is that the ramie fiber is removed, that is, only plastic fiber is used as the reinforcement material. The corresponding operation contents are omitted in the preparation method.

[0079] The test results of concrete properties are shown in Table 5. The test data show that after removing the ramie fiber from the reinforcement, the expansion rate of microcracks in the concrete matrix is ​​accelerated, resulting in the splitting tensile strength after curing for 28 days and the mechanical properties after 300 freeze-thaw cycles being lower than those in Example 1 to varying degrees.

[0080] Comparative Example 4

[0081] Reinforcement material comparison test 2, removing plastic fibers.

[0082] A concrete is prepared, and the same parts as those in Example 1 are not described in detail. The difference is that the plastic fiber is removed, that is, only ramie fiber is used as the reinforcement material. The corresponding operation contents are omitted in the preparation method.

[0083] The test results of concrete properties are shown in Table 5. The test data show that after removing the plastic fiber from the reinforcement, compared with Example 1, the splitting tensile strength of the concrete specimens after curing for 7 days, the splitting tensile strength at 28 days, and the compressive and splitting tensile strengths under freeze-thaw conditions are all reduced.

[0084] Comparative Example 5

[0085] Reinforcement Comparative Test 3, all reinforcements were removed.

[0086] A concrete is prepared, and the same parts as those in Example 1 are not described in detail. The difference is that all reinforcing materials are removed. The corresponding operations are omitted in the preparation method.

[0087] The concrete performance test results are shown in Table 5. The test data show that after removing all the reinforcing materials from the raw materials, the splitting strength and frost resistance durability of the concrete specimens after curing for different days are further reduced compared with Comparative Examples 3 and 4, indicating that the addition of the two fibers to the concrete helps to exert the synergistic effect of the two, thereby maximizing the frost resistance and anti-cracking performance of the specimens.

[0088] Comparative Example 6

[0089] Reinforcement material comparison test 4, flax replaces ramie.

[0090] A concrete is prepared, and the same parts as those in Example 1 are not described in detail. The difference is that in the reinforcing material, the ramie fiber is replaced by flax fiber of the same specification and mass fraction. The flax fiber is made of flax as a raw material and is prepared by the same processing method as the ramie fiber in Example 1.

[0091] The test results of concrete performance are shown in Table 5. The test data show that in the concrete component formula of the present invention, ramie fiber has a better effect on improving the anti-freezing and anti-cracking properties of concrete than flax.

[0092] Comparative Example 7

[0093] Reinforcement material comparison test 5, sisal replaces ramie.

[0094] A concrete is prepared, and the same parts as those in Example 1 are not repeated here. The difference is that the ramie fiber is replaced by sisal fiber of the same specification and mass fraction. The sisal fiber is made of sisal as raw material and is prepared by the same processing method as the ramie fiber in Example 1.

[0095] The test results of concrete performance are shown in Table 5. The test data show that in the concrete component formula of the present invention, the effect of ramie fiber on improving the anti-freezing and anti-cracking properties of concrete is better than that of sisal fiber.

[0096] Comparative Example 8

[0097] Reinforcement material comparison test 6, jute replacing ramie.

[0098] A concrete is prepared, and the same parts as those in Example 1 are not repeated here. The difference is that the ramie fiber is replaced by jute fiber of the same specification and mass fraction. The jute fiber is made of jute as raw material and is prepared by the same processing method as the ramie fiber in Example 1.

[0099] The concrete performance test results are shown in Table 5. The test data show that in the concrete component formula of the present invention, ramie fiber has a better effect on improving the anti-freezing and anti-cracking properties of concrete than jute.

[0100] Table 5 Concrete reinforcement material comparison test performance test results (unit: MPa)

[0101]

[0102]

[0103] Comparative Example 9

[0104] Admixture comparison test, removing admixture.

[0105] A concrete is prepared, and the same parts as those in Example 1 are not described in detail. The difference is that the admixture is removed. The corresponding operation contents are omitted in the preparation method.

[0106] The concrete performance test results are shown in Table 6. The test data show that without adding polycarboxylic acid high-performance water-reducing agent powder to the concrete components, the rough surface of the abandoned building stones absorbs too much free water during the mixing process, which is not conducive to the cement hydration reaction and limits the improvement of the frost resistance durability of the concrete specimens.

[0107] Table 6 Concrete admixture comparative test performance test results (unit: MPa)

[0108]

[0109] Comparative Example 10

[0110] Preparation method comparison test 1, exchanging the mixing process of admixtures, admixtures + binder materials.

[0111] A concrete is prepared, and the same points as those in Example 1 are not repeated here. The difference is that:

[0112] Step S100, add the admixture and 1 / 3 of the water into a No. 1 mixer, stir evenly (5 min to 8 min), and obtain a liquid high-efficiency water reducing agent;

[0113] Step S200: Add admixture and binder into mixer No. 1 and mix evenly (6 min to 9 min) to obtain a primary mixture.

[0114] The concrete performance test results are shown in Table 7. The test data show that the adjustment process is not conducive to cement modification.

[0115] Comparative Example 11

[0116] Preparation method comparison test 2, exchanging aggregate and admixture mixing process.

[0117] A concrete is prepared, and the same parts as those in the first embodiment are not repeated here. The difference is that after the modified cement-based material is prepared in step S100:

[0118] Step S200, putting the modified cement-based material, coarse aggregate and fine aggregate into a No. 1 mixer and stirring them evenly (6 min to 9 min) to obtain a primary mixture;

[0119] Step S300: Add additives and 1 / 3 of the amount of water into mixer No. 1, stir evenly (3 minutes to 4 minutes) to obtain a secondary mixture.

[0120] The test results of concrete performance are shown in Table 7. The test data show that the water-reducing efficiency of the water-reducing agent was not fully utilized after the adjustment process, resulting in a weakening of the antifreeze performance of the concrete after mixing and curing.

[0121] Comparative Example 12

[0122] Preparation method comparison test 3, combining the aggregate and reinforcing material mixing processes.

[0123] A concrete is prepared, and the same parts as those in the first embodiment are not described in detail. The difference is that after the primary mixture is prepared in step S200,

[0124] Step S300: Add coarse aggregate, fine aggregate, hemp fiber and plastic fiber into mixer No. 1 and mix them evenly (10 min to 15 min) to obtain a concrete mixture.

[0125] The concrete performance test results are shown in Table 7. The test data show that after the adjustment process, the three different material specifications of the multi-fibers contained in the reinforcement material failed to fully exert the bridging effect in the cracks of the concrete matrix.

[0126] Comparative Example 13

[0127] Preparation method comparison test 4 adopts a one-step mixing method.

[0128] A concrete was prepared, and the same parts as those in Example 1 are not described in detail, except that all raw materials were put into a mixer at one time and mixed evenly (44 min to 62 min).

[0129] The test results of concrete performance are shown in Table 7. The test data show that the anti-freezing and anti-cracking properties of the concrete specimens have significantly decreased.

[0130] Table 7 Concrete preparation method comparison test performance test results (unit: MPa)

[0131]

[0132] FIG2 is a schematic diagram comparing concrete preparation methods, wherein (a) to (e) are schematic diagrams of the preparation methods of Example 1, Comparative Example 10, Comparative Example 11, Comparative Example 12, and Comparative Example 13, respectively.

Claims

1. Environmentally friendly antifreeze and anti-cracking recycled concrete, the components include water, cementing material, coarse aggregate, fine aggregate, admixture, reinforcing material, admixture, the cementing material is cement, the admixture is a water reducing agent, characterized in that: The coarse aggregate includes crushed stone and recycled coarse aggregate, the fine aggregate is rock machine-made sand, the admixture is scallop shell powder, the reinforcing material includes hemp fiber and plastic fiber, and the plastic fiber includes plastic short fiber and plastic long fiber; the dosage of each component is: 150-180 parts of water, 370-420 parts of binder, 610-640 parts of coarse aggregate, 520-550 parts of fine aggregate, 40-70 parts of admixture, 55-60 parts of reinforcing material, and 13-17 parts of admixture.

2. The recycled concrete according to claim 1, characterized in that: The dosage of each component is one of the following schemes: 150 parts of water, 420 parts of cementitious materials, 610 parts of coarse aggregate, 520 parts of fine aggregate, 70 parts of admixture, 60 parts of reinforcing material, 17 parts of admixture, or, 160 parts of water, 400 parts of cementitious materials, 620 parts of coarse aggregate, 530 parts of fine aggregate, 60 parts of admixture, 55 parts of reinforcing material, 15 parts of admixture, or, 170 parts of water, 390 parts of cementitious materials, 630 parts of coarse aggregate, 540 parts of fine aggregate, 50 parts of admixture, 55 parts of reinforcing material, 14 parts of admixture, or, 180 parts of water, 370 parts of binder, 640 parts of coarse aggregate, 550 parts of fine aggregate, 40 parts of admixture, 60 parts of reinforcing material, and 13 parts of admixture.

3. The recycled concrete according to claim 1, characterized in that: The coarse aggregate, crushed stone and recycled coarse aggregate usage ratio is 1:1, the crushed stone particle size is 5 mm to 15 mm, and the recycled coarse aggregate particle size is 10 mm to 20 mm.

4. The recycled concrete according to claim 1, characterized in that: The reinforcing material comprises 10 to 40 parts of hemp fibers, 20 to 50 parts of plastic fibers, and the ratio of the plastic short fibers to the plastic long fibers is 2:

1.

5. The recycled concrete according to any one of claims 1 to 3, characterized in that: The rock machine-made sand is gneiss machine-made sand.

6. The recycled concrete according to any one of claims 1 to 3, characterized in that: The scallop shell powder is kitchen waste scallop shell powder with a particle size of 10 μm to 30 μm.

7. The concrete according to any one of claims 1 to 3, characterized in that: The hemp fiber is ramie fiber with a length of 15 mm to 25 mm and a diameter of 20 μm to 35 μm.

8. The recycled concrete according to any one of claims 1 to 3, characterized in that: The plastic fibers are processed from discarded plastic straws. The plastic short fibers have a length of 5 mm to 10 mm and a diameter of 100 μm to 150 μm. The plastic long fibers have a length of 15 mm to 20 mm and a diameter of 300 μm to 400 μm.

9. The recycled concrete according to any one of claims 1 to 3, characterized in that: The cement is ordinary Portland cement, and the water reducer is polycarboxylic acid high-performance FK-A type water reducer powder.

10. The method for preparing the environmentally friendly frost-resistant and crack-resistant recycled concrete according to any one of claims 1 to 8, characterized in that: First, prepare water, cementing materials, coarse aggregate, fine aggregate, admixtures, reinforcing materials, and admixtures according to the quantity and specifications, including: Scallop shell powder: Wash and disinfect kitchen waste scallop shells, dry them in an oven at 110℃~120℃, and grind them into powder; Hemp fiber: Hemp plants are treated with alkali and dried to make refined hemp fiber, which is then processed into fiber; Plastic fiber: The discarded straws are cleaned and disinfected, crushed and sheared into plastic short fibers and plastic long fibers, and then mixed evenly to obtain plastic fibers; Then mix the component raw materials according to the following steps: Step S100, mixing the admixture and the binder, dispersing by microwave and stirring evenly, to obtain a modified cement-based material; Step S200, putting the modified cement-based material, admixture and 1 / 3 of the water into a No. 1 mixer, stirring evenly to obtain a primary mixture; Step S300, continue to add coarse aggregate and fine aggregate, stir evenly, and obtain a secondary mixture; add hemp fiber and plastic fiber into the No. 2 mixer, stir evenly, and obtain a reinforcement material; Step S400, put the reinforcing material into mixer No. 1, add 1 / 3 of the amount of water, stir evenly, then add 1 / 3 of the amount of water, stir evenly, and obtain a concrete mixture.