Concrete for prefabricated column and preparation method thereof
By using cement, fly ash, steel slag, river sand, fiber and other components in prefabricated column concrete, and combining molybdenum boride and chromium carbide as modified fillers, the problem of insufficient strength and durability of prefabricated column concrete is solved, which is significantly It improves flexural strength and durability, and reduces the chloride ion diffusion coefficient.
Patent Information
- Application Number
- CN202411242897.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-05
- Publication Date
- 2024-11-08
AI Technical Summary
The existing concrete for prefabricated columns has low strength and poor durability, especially when it is subjected to large loads, which can easily accelerate the corrosion of metal supporting materials, affecting their durability.
Use cement, fly ash, steel slag, river sand, fiber and other components, and introduce molybdenum boride and chromium carbide as modified fillers. Through the combination of specific mass ratios and polymethylpentene, the strength and durability of concrete are improved. sex.
It significantly improves the flexural strength and durability of concrete, reduces the chloride ion diffusion coefficient, and meets higher durability requirements.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of concrete, and in particular to concrete for prefabricated columns and a preparation method thereof. Background Art
[0002] With the continuous advancement of building industrialization, prefabricated columns, as an efficient and high-quality building component, have a very broad application prospect. It can be combined with other prefabricated components to form a more complete prefabricated building system, which has made a great contribution to the sustainable development of the construction industry. Prefabricated columns are made of high-quality concrete raw materials, mixed according to the designed mix ratio, and then poured into the mold for proper maintenance. Because prefabricated columns often bear large loads in building structures, and the chloride ion diffusion coefficient of existing concrete is high, it will accelerate the corrosion of metal support materials, thereby affecting the durability of concrete prefabricated columns. Therefore, higher requirements are put forward for the strength and durability of concrete for prefabricated columns. The existing concrete for prefabricated columns still has the problems of low strength and poor durability, which need to be solved urgently. Summary of the invention
[0003] The present invention provides concrete for prefabricated columns and a preparation method thereof, which solves the problems of low concrete strength and poor durability in the related art.
[0004] The technical solution of the present invention is as follows: The present invention provides a concrete for prefabricated columns, comprising the following components in parts by weight: 80-90 parts of cement, 25-35 parts of fly ash, 14-24 parts of steel slag, 18-28 parts of modified filler, 10-15 parts of river sand, 12-16 parts of fiber, 55-65 parts of water, and 1-1.5 parts of water reducing agent; The modified filler comprises molybdenum boride and chromium carbide.
[0005] As a further technical solution, the mass ratio of the molybdenum boride to the chromium carbide is 1:11 to 11:1; Preferably, the mass ratio of the molybdenum boride to the chromium carbide is 2:3-5:1.
[0006] In the present invention, in the components of the modified filler, especially when the mass ratio of molybdenum boride to chromium carbide is 2:3-5:1, the strength and durability of the concrete are further improved.
[0007] As a further technical solution, the modified filler also includes polymethylpentene as a component.
[0008] As a further technical solution, the mass ratio of the molybdenum boride, chromium carbide and polymethylpentene is 2:3:0.1~0.5.
[0009] In the present invention, polymethylpentene is also introduced into the components of the modified filler. When the mass ratio of molybdenum boride, chromium carbide and polymethylpentene is 2:3:0.1-0.5, the durability of the concrete is further improved.
[0010] As a further technical solution, the preparation method of the modified filler comprises the following steps: S1, mixing polymethylpentene and molybdenum boride to obtain modified molybdenum boride; S2. Mixing the modified molybdenum boride, chromium carbide and coupling agent to obtain a modified filler.
[0011] As a further technical solution, step S1 specifically includes the following steps: after the polymethylpentene is melted, molybdenum boride is added to mix, cooled, and dispersed to obtain modified molybdenum boride.
[0012] As a further technical solution, the particle size of the steel slag is 30-80 μm; the particle size of the river sand is 0.25-0.5 mm; the diameter of the fiber is 50-100 μm, and the length is 4-8 mm.
[0013] As a further technical solution, the water reducer includes a lignin sulfonate water reducer and / or an aminosulfonate water reducer.
[0014] As a further technical solution, the fibers include organic fibers and / or inorganic fibers; the organic fibers include one or more of polyethylene fibers, polypropylene fibers, polyacrylonitrile fibers, lignin fibers, and polyester fibers; the inorganic fibers include one or more of glass fibers, basalt fibers, carbon fibers, and steel fibers.
[0015] The present invention also proposes a method for preparing concrete for prefabricated columns, comprising the following steps: After the components of the concrete are mixed, concrete is obtained.
[0016] The present invention also proposes the use of the concrete for prefabricated columns or the concrete prepared by the preparation method on prefabricated columns of assembled buildings.
[0017] The working principle and beneficial effects of the present invention are: In the present invention, the concrete adopts cement, fly ash, steel slag, river sand, fiber and other components, and simultaneously introduces molybdenum boride and chromium carbide as modified fillers to synergistically enhance the concrete matrix, thereby significantly improving the strength and durability of the concrete. DETAILED DESCRIPTION
[0018] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0019] In the following examples and comparative examples, the type of cement is ordinary Portland cement PO 32.5; the particle size of chromium carbide is 15-45 μm, and the average particle size is 32 μm; the particle size of molybdenum boride is 5-10 μm, and the average particle size is 6 μm; and the type of polymethylpentene is MX002.
[0020] Example 1 The concrete for prefabricated columns comprises the following components in parts by weight: 80 parts of cement, 25 parts of secondary fly ash, 14 parts of steel slag (particle size 30 μm), 18 parts of modified filler, 10 parts of river sand (particle size 0.25-0.5 mm, average particle size 0.3 mm), 6 parts of glass fiber (diameter 100 μm, length 4 mm), 6 parts of basalt fiber (diameter 100 μm, length 4 mm), 55 parts of water, and 1 part of potassium lignin sulfonate; wherein the modified filler is molybdenum boride and chromium carbide in a mass ratio of 11:1; The method for preparing concrete for precast columns comprises the following steps: After the components of concrete are mixed, concrete is obtained.
[0021] Example 2 The concrete for prefabricated columns comprises the following components in parts by weight: 90 parts of cement, 35 parts of secondary fly ash, 24 parts of steel slag (particle size 80 μm), 28 parts of modified filler, 15 parts of river sand (particle size 0.25-0.5 mm, average particle size 0.3 mm), 16 parts of glass fiber (diameter 50 μm, length 6 mm), 65 parts of water, and 1.5 parts of potassium lignin sulfonate; wherein the modified filler is molybdenum boride and chromium carbide in a mass ratio of 1:11; The method for preparing concrete for precast columns comprises the following steps: After the components of concrete are mixed, concrete is obtained.
[0022] Example 3 The concrete for prefabricated columns comprises the following components in parts by weight: 85 parts of cement, 30 parts of secondary fly ash, 18 parts of steel slag (particle size 50 μm), 24 parts of modified filler, 12 parts of river sand (particle size 0.25-0.5 mm, average particle size 0.3 mm), 7 parts of basalt fiber (diameter 100 μm, length 8 mm), 6 parts of polypropylene fiber (diameter 100 μm, length 4 mm), 60 parts of water, and 1 part of potassium lignin sulfonate; wherein the modified filler is molybdenum boride and chromium carbide in a mass ratio of 1:3; The method for preparing concrete for precast columns comprises the following steps: After the components of concrete are mixed, concrete is obtained.
[0023] Example 4 The only difference between this embodiment and embodiment 3 is that the modified filler is molybdenum boride and chromium carbide in a mass ratio of 7:1.
[0024] Example 5 The only difference between this embodiment and embodiment 3 is that the modified filler is molybdenum boride and chromium carbide in a mass ratio of 5:1.
[0025] Example 6 The only difference between this embodiment and embodiment 3 is that the modified filler is molybdenum boride and chromium carbide in a mass ratio of 2:3.
[0026] Example 7 The only difference between this embodiment and embodiment 6 is that the modified filler is molybdenum boride, chromium carbide, and polymethylpentene in a mass ratio of 2:3:0.6.
[0027] Example 8 The difference between this embodiment and embodiment 6 is that the modified filler is molybdenum boride, chromium carbide, and polymethylpentene in a mass ratio of 2:3:0.6, and the preparation method of the modified filler comprises the following steps: S1. After melting polymethylpentene, add molybdenum boride to mix, cool, and disperse to obtain modified molybdenum boride; S2, mixing modified molybdenum boride, chromium carbide and coupling agent KH580 to obtain a modified filler; The coupling agent KH580 was dissolved in 70% ethanol by volume before mixing, the mass volume ratio of the coupling agent KH580 to ethanol was 1 g:20 mL, and the mass ratio of chromium carbide to the coupling agent KH580 was 1:0.2.
[0028] Example 9 The only difference between this embodiment and embodiment 8 is that the modified filler is molybdenum boride, chromium carbide, and polymethylpentene in a mass ratio of 2:3:0.08.
[0029] Example 10 The only difference between this embodiment and embodiment 8 is that the modified filler is molybdenum boride, chromium carbide, and polymethylpentene in a mass ratio of 2:3:0.1.
[0030] Embodiment 11 The only difference between this embodiment and embodiment 8 is that the modified filler is molybdenum boride, chromium carbide, and polymethylpentene in a mass ratio of 2:3:0.5.
[0031] Comparative Example 1 The difference between this comparative example and Example 3 is that the modified filler is molybdenum boride.
[0032] Comparative Example 2 The only difference between this comparative example and Example 3 is that the modified filler is chromium carbide.
[0033] Comparative Example 3 The only difference between this comparative example and Example 3 is that no modified filler is added.
[0034] Comparative Example 4 The only difference between this comparative example and Example 3 is that the modified filler is polymethylpentene.
[0035] The strength and durability tests were performed on the concretes obtained in Examples 1 to 11 and Comparative Examples 1 to 4 respectively: Strength: 28d flexural strength test is carried out in accordance with the standard GB / T 50081-2019 "Test methods for physical and mechanical properties of concrete"; Durability: According to the standard GB / T50476-2019 "Concrete Structure Durability Design Code", the chloride ion diffusion coefficient test at 28 days is carried out. Among them, the chloride ion intrusion resistance index of concrete (design service life is 100 years, environmental action level E) should meet the following requirements: the chloride ion diffusion coefficient should be ≤4×10 -12 m 2 / s.
[0036] The results are shown in Table 1 below.
[0037] Table 1 Concrete performance test results
[0038] By comparing the data of Examples 1 to 11 and Comparative Examples 1 to 4, it is found that compared with Comparative Examples 1 to 4, the concrete prepared in Examples 1 to 11 has higher flexural strength and smaller chloride ion diffusion coefficient, indicating that the concrete uses cement, fly ash, steel slag, river sand, fiber and other components, and introduces molybdenum boride and chromium carbide as modified fillers, which can significantly improve the strength and durability of the concrete.
[0039] By comparing the data of Examples 3 to 6, it is found that compared with Examples 3 to 4, the concrete prepared in Examples 5 to 6 has higher flexural strength and smaller chloride ion diffusion coefficient, indicating that the components of the modified filler, especially when the mass ratio of molybdenum boride to chromium carbide is 2:3 to 5:1, further improve the strength and durability of the concrete.
[0040] By comparing the data of Examples 6 to 11, it is found that compared with Examples 6 to 7, the concrete prepared in Examples 8 to 11 has higher flexural strength and smaller chloride ion diffusion coefficient, indicating that the components of the modified filler also introduce polymethylpentene, and molybdenum boride and chromium carbide are combined to further improve the strength and durability of the concrete; compared with Examples 8 to 9, the concrete prepared in Examples 10 to 11 has higher flexural strength and smaller chloride ion diffusion coefficient, indicating that especially when the mass ratio of molybdenum boride, chromium carbide and polymethylpentene is 2:3:0.1 to 0.5, the durability of the concrete can be further improved.
[0041] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A concrete for precast columns, characterized in that: The invention comprises the following components in parts by weight: 80-90 parts of cement, 25-35 parts of fly ash, 14-24 parts of steel slag, 18-28 parts of modified filler, 10-15 parts of river sand, 12-16 parts of fiber, 55-65 parts of water, and 1-1.5 parts of water reducing agent; The modified filler comprises molybdenum boride and chromium carbide.
2. The concrete for precast columns according to claim 1, characterized in that: The mass ratio of molybdenum boride to chromium carbide is 1:11 to 11:1; Preferably, the mass ratio of the molybdenum boride to the chromium carbide is 2:3-5:
1.
3. The concrete for precast columns according to claim 1, characterized in that: The modified filler also includes polymethylpentene as a component.
4. The concrete for precast columns according to claim 3, characterized in that: The mass ratio of the molybdenum boride, chromium carbide and polymethylpentene is 2:3:0.1-0.
5.
5. The concrete for precast columns according to claim 4, characterized in that: The preparation method of the modified filler comprises the following steps: S1, mixing polymethylpentene and molybdenum boride to obtain modified molybdenum boride; S2. Mixing the modified molybdenum boride, chromium carbide and coupling agent to obtain a modified filler.
6. The concrete for precast columns according to claim 1, characterized in that: The particle size of the steel slag is 30-80 μm; the particle size of the river sand is 0.25-0.5 mm; the diameter of the fiber is 50-100 μm, and the length is 4-8 mm.
7. The concrete for precast columns according to claim 1, characterized in that: The water reducer includes a lignin sulfonate water reducer and / or an aminosulfonate water reducer.
8. The concrete for precast columns according to claim 1, characterized in that: The fibers include organic fibers and / or inorganic fibers; the organic fibers include one or more of polyethylene fibers, polypropylene fibers, polyacrylonitrile fibers, lignin fibers, and polyester fibers; the inorganic fibers include one or more of glass fibers, basalt fibers, carbon fibers, and steel fibers.
9. A method for preparing concrete for precast columns according to any one of claims 1 to 8, characterized in that: The following steps are involved: After the components of the concrete are mixed, concrete is obtained.
10. Use of the concrete for prefabricated columns according to any one of claims 1 to 8 or the concrete prepared by the preparation method according to claim 9 in prefabricated columns of assembled buildings.