Preparation method of slow-release fertilizer hydrogel

By loading urea on the Elostone nanotubes and grafting isocyanate to form a hydrogel system, the problems of Elostone nanoparticles agglomeration and insufficient mechanical strength of the hydrogel are solved, and better fertilizer slow release and soil structure are achieved improve.

CN118908773AInactive Publication Date: 2024-11-08DONGGUAN LUCKY CHEM CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411002266.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-11-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Elostone nanoparticles are prone to agglomeration, resulting in poor sustained release effect. The lack of mechanical strength of traditional hydrogels limits its wider application.

Method used

By loading urea into elostear nanotubes and grafting isocyanate on the surface of elostear nanotubes to form a single-network or double-network hydrogel system, it increases mechanical properties and achieves better fertilizer sustained release effect.

Benefits of technology

It improves the adsorption and sustained release effect of urea, enhances the mechanical properties of the hydrogel, achieves more uniform dispersion of Elosite nanotubes and better slow release of fertilizers, improving soil structure and water and fertilizer utilization.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004961917010000081
    Figure BDA0004961917010000081
Patent Text Reader

Abstract

The invention relates to a preparation method of slow-release fertilizer hydrogel, and belongs to the technical field of fertilizers, the preparation method comprises the following steps: S1, dispersing halloysite nanotubes in a urea solution under ultrasound, filtering and drying to obtain halloysite nanotube loaded urea; and S2, grafting isocyanate on the surface of the halloysite nanotube-loaded urea, mixing with acrylamide and sodium carboxymethyl cellulose, adding an initiator to obtain a suspension, dropwise adding the obtained suspension into a metal salt solution, and reacting to obtain the slow-release fertilizer hydrogel. According to the technical scheme, urea is loaded into halloysite nanotubes, then isocyanate is grafted to the surfaces of the halloysite nanotubes, then the halloysite nanotubes and acrylamide form a single-network hydrogel system, and a double-network hydrogel system is formed through ionic crosslinking between sodium carboxymethyl cellulose and A ions, so that the mechanical property of the hydrogel is improved; and a better slow-release effect of the fertilizer is also realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of concrete, and in particular relates to a method for preparing a low-density polyethylene antioxidant packaging film. Background Art

[0002] As the main source of crop growth, fertilizer has made an important contribution to agricultural production and is also a key factor in the sustainable development of agriculture. At the same time, fertilizer and water improve the vitality of crops. Fertilization of crops can effectively increase the growth of crops and improve production efficiency, and fertilization has a high contribution rate to crop yield. However, 30-70% of the nutrients in conventional fertilizers are released into the environment, causing serious environmental pollution. Therefore, the development of slow-release fertilizers is an effective way to maintain fertilizer concentration, reduce nutrient loss, and promote stable crop growth. Improving fertilizer utilization and reducing fertilizer pollution to the land environment are currently important research topics. However, there are still many problems to be solved in the field of slow-release fertilizer research. Due to the high cost of fertilizers, the release rate of fertilizers is inconsistent with the growth needs of crops, and the efficiency of fertilizer use is greatly reduced.

[0003] In order to reduce the cost of fertilizers and their impact on the environment, fertilizers made from non-toxic, biocompatible, abundant and relatively cheap natural materials such as natural polysaccharides and clays have received widespread attention. Halloysite nanotubes are an attractive natural one-dimensional nanomaterial with a hollow tubular nanostructure, a high aspect ratio and a differential structure between the inner and outer surfaces, which can effectively load fertilizers. However, the nanostructured particles are prone to agglomeration, resulting in poor sustained release effects. Hydrogels are three-dimensional polymers that can absorb and retain large amounts of water or aqueous solutions. However, most traditional hydrogels have inherently poor mechanical strength, which limits their wider application. Summary of the invention

[0004] The object of the present invention is to provide a method for preparing a slow-release fertilizer hydrogel, by loading urea into halloysite nanotubes, grafting isocyanate on the surface of the halloysite nanotubes, and then forming a single-network hydrogel system with acrylamide, and forming a double-network hydrogel system through ionic crosslinking between sodium carboxymethyl cellulose and Al ions, thereby increasing the mechanical properties of the hydrogel and achieving a better slow-release effect of the fertilizer.

[0005] Technical problems to be solved by the present invention: Although halloysite nanoparticles can adsorb urea, they are easy to agglomerate, resulting in poor sustained release effect; hydrogels are three-dimensional polymers that can absorb and retain large amounts of water or aqueous solutions, however, most traditional hydrogels have inherently poor mechanical strength, which limits their wider application.

[0006] The purpose of the present invention can be achieved through the following technical solutions:

[0007] A method for preparing a slow-release fertilizer hydrogel comprises the following steps:

[0008] S1, dispersing the halloysite nanotubes in a urea solution under ultrasound, and obtaining urea loaded with the halloysite nanotubes after filtering and drying;

[0009] S2, grafting isocyanate on the surface of urea supported by halloysite nanotubes, mixing with acrylamide and sodium carboxymethyl cellulose, adding an initiator to obtain a suspension, and dropping the obtained suspension into a metal salt solution. After the reaction is completed, a slow-release fertilizer hydrogel is obtained;

[0010] Urea forms hydrogen bonds with the surface of halloysite nanotubes to achieve loading of urea on the halloysite nanotubes; 2-ethyl isocyanate is grafted onto the surface of the urea loaded on the halloysite nanotubes to fix vinyl groups on the surface of the halloysite nanotubes through a click reaction between NCO groups and OH groups to achieve surface modification of the halloysite nanotubes; the surface-modified halloysite nanotubes are mixed with acrylamide, an initiator and sodium carboxymethyl cellulose, and a slow-release fertilizer hydrogel is prepared through polymerization initiated by the initiator and chelation of the sodium carboxymethyl cellulose with metal ions in a metal salt solution during the polymerization process;

[0011] Further, the urea loaded by the halloysite nanotubes is prepared by the following steps:

[0012] Urea and deionized water are added to a 250 mL reactor containing halloysite nanotubes, reacted at 135° C. for 4 hours, and dried to obtain a product, wherein the amount of urea, deionized water and halloysite nanotubes is 3-5 g: 90-110 mL: 15-25 g.

[0013] Further, the surface grafting of isocyanate comprises the following steps:

[0014] The surface grafted isocyanate is mixed with acrylamide and is prepared by the following steps:

[0015] A1: dissolving urea loaded with halloysite nanotubes and 2-isocyanatoethyl methacrylate in anhydrous dimethyl sulfoxide, stirring evenly, and heating at 70°C for 12 hours to form a mixture, cooling the mixture to room temperature, and then washing it with acetone and methanol for three times, and filtering it to obtain the mixture; wherein the amount of halloysite nanotubes, 2-isocyanatoethyl methacrylate and anhydrous dimethyl sulfoxide is 90-110 mg: 480-520 mg: 1-3 mL;

[0016] A2: Halloysite nanotubes with surface grafted isocyanate, acrylamide and sodium carboxymethyl cellulose are added to deionized water and mixed. After the vial is degassed by purging with argon for 10 minutes, ammonium persulfate is added and stirred to form a suspension, wherein the amount of Halloysite nanotubes with surface grafted isocyanate, acrylamide, sodium carboxymethyl cellulose, deionized water and ammonium persulfate is 40-60 mg: 200-210 g: 50-70 mg: 90-110 mL: 25-35 mg.

[0017] Further, the step of adding the suspension dropwise to the aluminum chloride solution comprises the following steps:

[0018] The suspension was dripped into the aluminum chloride solution with a syringe, stirred magnetically, and the product was filtered after standing for 20 minutes, and the temperature was raised to 60°C to continue the polymerization reaction for 3 hours, and then washed with deionized water and dried in a vacuum oven at 70°C to obtain the product. The amount of the suspension, aluminum chloride solution and deionized water was 40-60mL: 40-60mL: 90-110mL.

[0019] In the above reaction process, the urea loaded on the halloysite nanotubes undergoes a click reaction between the -OH group on the surface and the -NCO group in 2-isocyanatoethyl methacrylate to fix the vinyl group on the surface of the halloysite nanotubes, and then polymerizes with acrylamide under the initiation of the initiator ammonium persulfate. During this polymerization process, due to the addition of sodium carboxymethyl cellulose, after the suspension is dropped into the aluminum chloride solution, a metal-carboxylate coordination bond is formed between the sodium carboxymethyl cellulose and the aluminum ions to form a double network hydrogel.

[0020] Beneficial effects of the present invention:

[0021] (1) In the technical scheme of the present invention, urea loaded on halloysite nanotubes is prepared by forming hydrogen bonds between urea and the surface of halloysite nanotubes. On the one hand, the halloysite nanotubes have a higher specific surface area, which increases the adsorption of urea and achieves a better sustained release effect of urea. On the other hand, the inner surface of the halloysite nanotubes is positively charged, which combines with the negative charge carried by the soil to further achieve the controlled release of urea. The surface of the urea loaded on the halloysite nanotubes is grafted with 2-ethyl isocyanate methacrylate, and the vinyl group is fixed on the surface of the halloysite nanotubes through a click reaction between the -NCO group and the -OH group to achieve surface modification of the halloysite nanotubes. The subsequently formed hydrogel structure uses the halloysite nanotubes as connection points, achieves directional arrangement of the halloysite nanotubes, reduces the agglomeration of the halloysite nanotubes, and achieves slow release of urea adsorbed in the uniformly dispersed halloysite nanotubes in the hydrogel.

[0022] (2) In the technical scheme of the present invention, ammonium persulfate is used to bond sodium carboxymethyl cellulose to the surface active functional groups of halloysite nanotubes, and electrostatic interaction occurs between carboxyl groups and aluminum ions to form metal-carboxylic acid coordination bonds, thereby forming a double-network structured hydrogel system. Since water is essential for the growth of crops, it can also help crops absorb fertilizers. Water and fertilizer interact and influence each other to jointly promote crop growth. The hydrogel has a three-dimensional polymer network that can absorb and retain a large amount of aqueous solution, making full use of water sources. The hydrogel can not only reduce the frequency of irrigation and prevent water loss, but also promote the formation of soil aggregates and improve soil structure. When plant growth requires nutrients, the nutrients absorbed by the hydrogel from the soil are released through exchange interactions. The double-network structured hydrogel system has more excellent mechanical properties, including high toughness, high anti-destruction and high water content. The double-network system cooperates with the nanoparticle structure of the halloysite nanotubes to achieve a superimposed effect on the slow release of urea. DETAILED DESCRIPTION

[0023] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0024] The use process of the dispersant is as follows: the fiber is first hydrophobically modified with a hydrophobic modifier, then modified with a surfactant, then loaded with anionic clay, and then mixed with foamed concrete.

[0025] Example 1

[0026] A method for preparing a slow-release fertilizer hydrogel comprises the following steps:

[0027] A1. Add 3 g urea and 90 mL deionized water into a 250 mL reactor containing 15 g halloysite nanotubes, react at 135 °C for 4 h, and obtain urea loaded with halloysite nanotubes after filtration and drying;

[0028] A2, 90 mg of urea loaded with halloysite nanotubes and 480 mg of 2-isocyanatoethyl methacrylate were dispersed in 10 mL of anhydrous dimethyl sulfoxide, stirred evenly, and heated at 70° C. for 12 h to form a mixture, cooled the mixture to room temperature, and then washed with acetone and methanol for 3 times, and filtered to obtain;

[0029] A3, 40 mg of the surface-grafted isocyanate halloysite nanotubes, 200 mg of acrylamide and 50 mg of sodium carboxymethyl cellulose were added to 90 mL of deionized water for mixing, and the vial was degassed by purging with argon for 10 minutes, and then 25 mg of ammonium persulfate was added and stirred to form a suspension;

[0030] A4. Add 40 mL of the suspension into 40 mL of aluminum chloride solution with a syringe, stir magnetically, filter the product after standing for 20 min, raise the temperature to 60 ° C and continue the polymerization reaction for 3 h, wash with 90 mL of deionized water, and dry in a vacuum oven at 70 ° C to obtain the finished product.

[0031] Example 2

[0032] A method for preparing a slow-release fertilizer hydrogel comprises the following steps:

[0033] A1. Add 4 g urea and 100 mL deionized water into a 250 mL reactor containing 20 g halloysite nanotubes, react at 135° C. for 4 h, and obtain urea loaded with halloysite nanotubes after filtration and drying;

[0034] A2, dispersing 100 mg of urea loaded with halloysite nanotubes and 500 mg of 2-isocyanatoethyl methacrylate in 20 mL of anhydrous dimethyl sulfoxide, stirring evenly, and heating at 70° C. for 12 h to form a mixture, cooling the mixture to room temperature, and then washing with acetone and methanol for three times, and filtering to obtain;

[0035] A3, 50 mg of the surface-grafted isocyanate halloysite nanotubes, 205 mg of acrylamide and 60 mg of sodium carboxymethyl cellulose were added to 100 mL of deionized water for mixing, and after the vial was degassed by purging with argon for 10 minutes, 30 mg of ammonium persulfate was added and stirred to form a suspension;

[0036] A4. Add 50 mL of the suspension into 50 mL of aluminum chloride solution with a syringe and stir magnetically. After standing for 20 min, filter the product, raise the temperature to 60 ° C and continue the polymerization reaction for 3 h. After washing with 100 mL of deionized water, dry it in a vacuum oven at 70 ° C to obtain the finished product.

[0037] Example 3

[0038] A method for preparing a slow-release fertilizer hydrogel comprises the following steps:

[0039] A1. Add 5 g urea and 110 mL deionized water into a 250 mL reactor containing 25 g halloysite nanotubes, react at 135 °C for 4 h, and obtain urea loaded with halloysite nanotubes after filtration and drying;

[0040] A2, 110 mg of urea loaded with halloysite nanotubes and 520 mg of 2-isocyanatoethyl methacrylate were dispersed in 30 mL of anhydrous dimethyl sulfoxide, stirred evenly, and heated at 70° C. for 12 h to form a mixture, cooled the mixture to room temperature, and then washed with acetone and methanol for three times, and filtered to obtain;

[0041] A3, 60 mg of the surface-grafted isocyanate halloysite nanotubes, 210 mg of acrylamide and 70 mg of sodium carboxymethyl cellulose were added to 110 mL of deionized water for mixing, and the vial was degassed by purging with argon for 10 minutes, and then 35 mg of ammonium persulfate was added and stirred to form a suspension;

[0042] A4. Add 60 mL of the suspension into 60 mL of aluminum chloride solution with a syringe, stir magnetically, filter the product after standing for 20 min, raise the temperature to 60 ° C and continue the polymerization reaction for 3 h, wash with 110 mL of deionized water, and dry in a vacuum oven at 70 ° C to obtain the finished product.

[0043] Comparative Example 1

[0044] A method for preparing a slow-release fertilizer hydrogel comprises the following steps:

[0045] A1. Add 5 g urea and 110 mL deionized water into a 250 mL reactor containing 25 g halloysite nanotubes, react at 135 °C for 4 h, and obtain urea loaded with halloysite nanotubes after filtration and drying;

[0046] A2, 110 mg of urea loaded with halloysite nanotubes, 520 mg of 2-isocyanatoethyl methacrylate, 210 mg of acrylamide and 70 mg of sodium carboxymethyl cellulose were added to 110 mL of deionized water and mixed, and after degassing the vial with argon for 10 minutes, 35 mg of ammonium persulfate was added and stirred to form a suspension;

[0047] A3. Add 60 mL of the suspension into 60 mL of aluminum chloride solution with a syringe, stir magnetically, filter the product after standing for 20 min, raise the temperature to 60 ° C and continue the polymerization reaction for 3 h, wash with 110 mL of deionized water, and dry in a vacuum oven at 70 ° C to obtain the finished product.

[0048] Comparative Example 2

[0049] A method for preparing a slow-release fertilizer hydrogel comprises the following steps:

[0050] A1. Add 5 g urea and 110 mL deionized water into a 250 mL reactor containing 25 g halloysite nanotubes, react at 135 °C for 4 h, and obtain urea loaded with halloysite nanotubes after filtration and drying;

[0051] A2, 110 mg of urea loaded with halloysite nanotubes and 520 mg of 2-isocyanatoethyl methacrylate were dispersed in 30 mL of anhydrous dimethyl sulfoxide, stirred evenly, and heated at 70° C. for 12 h to form a mixture, cooled the mixture to room temperature, and then washed with acetone and methanol for three times, and filtered to obtain;

[0052] A3. 60 mg of the surface-grafted isocyanate halloysite nanotubes and 210 mg of acrylamide were added to 110 mL of deionized water and mixed. After the vial was degassed by purging with argon for 10 minutes, 35 mg of ammonium persulfate was added. After the reaction was completed, the finished product was obtained.

[0053] The slow-release fertilizer hydrogel prepared in Example 1-3 and Comparative Example 1-2 is now subjected to performance testing, and the testing process is as follows: First, two PVC tubes (10 cm in diameter and 30 cm in height) are sealed with 200 mesh nylon cloth. Secondly, a mixture of dry sand (100 g) and a dry sample (1 g) is placed in a PVC tube. Another PVC tube containing dry sand (100 g) and not containing WSF is used as a control. Afterwards, 70 mL of distilled water is poured into each PVC tube at predetermined time intervals, and the leachate is collected in a flask below the bottom of the PVC tube. The urea concentration of the soil leachate is determined by spectrophotometry, and the test results are shown in Table 1 below.

[0054] Table 1

[0055]

[0056] It can be seen from Table 1 above that by loading urea into halloysite nanotubes, grafting isocyanate on the surface of halloysite nanotubes, and then forming a single-network hydrogel system with acrylamide, a double-network hydrogel system is formed through ionic crosslinking between sodium carboxymethyl cellulose and Al ions, which increases the mechanical properties of the hydrogel and achieves a better sustained-release effect of the fertilizer.

[0057] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0058] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.

Claims

1. A method for preparing a slow-release fertilizer hydrogel, characterized in that: The following steps are involved: S1, dispersing the halloysite nanotubes in a urea solution under ultrasound, and obtaining urea loaded with the halloysite nanotubes after filtering and drying; S2, grafting isocyanate on the surface of urea supported by halloysite nanotubes, mixing with acrylamide and sodium carboxymethyl cellulose, adding an initiator to obtain a suspension, and dropping the obtained suspension into a metal salt solution. After the reaction is completed, a slow-release fertilizer hydrogel is obtained; Urea forms hydrogen bonds with the surface of halloysite nanotubes to achieve the loading of urea on the halloysite nanotubes; 2-ethyl isocyanate is grafted onto the surface of the urea loaded on the halloysite nanotubes to fix the vinyl group on the surface of the halloysite nanotubes through a click reaction between the -NCO group and the -OH group to achieve the surface modification of the halloysite nanotubes; the surface-modified halloysite nanotubes are mixed with acrylamide, an initiator and sodium carboxymethyl cellulose, and a slow-release fertilizer hydrogel is prepared through the initiation polymerization of the initiator and the chelation effect between the sodium carboxymethyl cellulose and the metal ions in the metal salt solution during the polymerization process.

2. The method for preparing a slow-release fertilizer hydrogel according to claim 1, characterized in that: The initiator is ammonium persulfate.

3. The method for preparing a slow-release fertilizer hydrogel according to claim 1, characterized in that: The urea supported by the halloysite nanotubes is prepared by the following steps: Urea and deionized water were added into a reactor containing halloysite nanotubes, and reacted at 135° C. for 4 hours. After filtering and drying, urea loaded with halloysite nanotubes was obtained.

4. The method for preparing a slow-release fertilizer hydrogel according to claim 2, characterized in that: The dosage of urea, deionized water and halloysite nanotubes is 3-5 g: 90-110 mL: 15-25 g.

5. The method for preparing a slow-release fertilizer hydrogel according to claim 1, characterized in that: The surface grafting of isocyanate and acrylamide is mixed and comprises the following steps: A1. Dispersing urea loaded on halloysite nanotubes and 2-isocyanatoethyl methacrylate in anhydrous dimethyl sulfoxide, stirring evenly, and heating at 70° C. for 12 h to form a mixture, cooling the mixture to room temperature, and then washing it with acetone and methanol for three times, and filtering to obtain halloysite nanotubes with surface grafted with isocyanate; A2. The halloysite nanotubes with surface grafted with isocyanate, acrylamide and sodium carboxymethyl cellulose were added to deionized water and mixed. After the vial was degassed by purging with argon for 10 minutes, ammonium persulfate was added and stirred to form a suspension.

6. The method for preparing a slow-release fertilizer hydrogel according to claim 5, characterized in that: In step A1, the amount of urea, 2-isocyanatoethyl methacrylate and anhydrous dimethyl sulfoxide loaded on the halloysite nanotubes is 90-110 mg: 480-520 mg: 10-30 mL; In step A2, the amounts of the halloysite nanotubes with isocyanate grafted on the surface, acrylamide, sodium carboxymethyl cellulose, deionized water and ammonium persulfate are 40-60 mg: 200-210 mg: 50-70 mg: 90-110 mL: 25-35 mg.

7. The method for preparing a slow-release fertilizer hydrogel according to claim 1, characterized in that: The metal salt solution is aluminum chloride solution.

8. The method for preparing a slow-release fertilizer hydrogel according to claim 1, characterized in that: The step of adding the suspension dropwise to the aluminum chloride solution comprises the following steps: The suspension was dripped into the aluminum chloride solution with a syringe and stirred magnetically. After standing for 20 minutes, the product was filtered, the temperature was raised to 60°C and the polymerization reaction was continued for 3 hours. After washing with deionized water, the product was dried in a vacuum oven at 70°C to obtain the finished product.