Continuous mixing safety production method for explosives and powders

By using non-energy-containing powder materials in continuous mixing equipment for fire explosives, the safety hazards of not mixing completely fire explosives slurry during the equipment cleaning process are solved, and the effect of reducing the risk of manual cleaning is achieved, ensuring the fire Safety of explosives production.

CN118908793APending Publication Date: 2024-11-08XIAN MODERN CHEM RES INST
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411027036.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

In continuous mixing of fire explosives, a large amount of fire explosives slurry that is not completely mixed during the equipment cleaning process, resulting in safety hazards and affecting production safety.

Method used

Use non-energy-containing powder materials (such as anhydrous sodium sulfate, anhydrous potassium sulfate, and anhydrous calcium carbonate) as substitutes to safely clean the energy-containing components of the residual ignition-explosive continuous mixing equipment to reduce labor Clean up the danger.

Benefits of technology

It effectively reduces the danger during manual cleaning, avoids the occurrence of safety accidents, protects the safety of people's lives and property, and meets the safety needs of ignition explosives production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118908793A_ABST
    Figure CN118908793A_ABST
Patent Text Reader

Abstract

The invention provides an explosive and powder continuous mixing safety production method, which comprises the following steps of: after one-time explosive and powder mixing operation is finished, safely cleaning explosive and powder continuous mixing equipment by using a non-energetic powder material as a substitute material, and then carrying out next-time explosive and powder mixing operation. According to the invention, the non-energetic substitute material is utilized to extrude a large amount of dangerous waste which is remained in the chamber and is not in a completely mixed state, so that only a small amount of material which is adhered to the paddle and the wall surface of the chamber is remained in the mixing equipment, and at the moment, the content of energetic components in the residual material is obviously lower than that of the mixed material before the substitute material is extruded; therefore, the danger in the manual cleaning process is greatly reduced, safety accidents are avoided, the life and property safety of personnel is guaranteed, and the requirement of current explosive and powder production for safety supply is met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of explosive and pyrotechnic products, relates to a continuous mixing technology of explosive and pyrotechnics, and specifically relates to a safe production method for continuous mixing of explosive and pyrotechnics. Background Art

[0002] Kneading and mixing of energetic materials is a common process in the production and charging of explosives such as PBX explosives and solid propellants. In traditional production, this process is mainly completed by vertical kneading machines. With the continuous development of new energetic materials and the continuous improvement of product performance requirements, the types and solid content of high-viscosity composite materials in explosives have increased. In addition, the current demand for weapons and ammunition is also increasing, which puts higher requirements on the kneading capacity, material application range, mixing efficiency, etc. of existing kneading technology.

[0003] The Chinese patent application number CN202011202790.3 discloses a multi-chamber continuous kneading machine for kneading and mixing energetic materials. Compared with the traditional vertical kneading machine, it has the advantages of strong kneading ability, high efficiency, continuous operation, good product adaptability, etc., and has very good prospects for promotion and application. However, for the continuous explosive mixing method, after completing a single shift, the mixing chamber is still filled with a large amount of unmixed explosive slurry. These slurries are not only unable to be loaded as qualified products, but the high content of energetic materials in them also brings great safety hazards to the cleaning of the chamber, especially in the upstream chamber. There are a large number of uncoated energetic powder materials, whose sensitivity is much higher than that of the mixed explosive product slurry.

[0004] At present, the multi-chamber continuous mixing charging method has realized the automation and unmanned process of adding, mixing and pouring. However, the cleaning of the chamber after a single shift still requires the participation of operators on site, which is very dangerous. This has a certain impact on ensuring the safe production of multi-chamber continuous mixing charging and has become one of the bottlenecks restricting the development of this technology. Summary of the invention

[0005] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a method for safe production of continuous mixing of explosives and propellants, so as to solve the technical problem in the prior art that during the continuous mixing production of explosives and propellants, a large amount of incompletely mixed explosive slurry is likely to cause safety accidents during the cleaning of equipment by personnel between shifts.

[0006] In order to solve the above technical problems, the present invention adopts the following technical solutions to achieve the above problems:

[0007] A method for safe production of continuous mixing of explosives and propellants, the method comprising: after a mixing operation of explosives and propellants is completed, non-energetic powder materials are used as substitute materials to safely clean up the energetic components of explosives and propellants remaining in a continuous mixing device of explosives and propellants, and then the next mixing operation of explosives and propellants is carried out.

[0008] The non-energetic powder material is selected from one or more of anhydrous sodium sulfate, anhydrous potassium sulfate and anhydrous calcium carbonate.

[0009] The energetic components of the explosive are selected from one or more of RDX, ammonium perchlorate and octogenin.

[0010] The present invention also has the following technical features:

[0011] The explosive continuous mixing equipment comprises a multi-chamber continuous kneading machine, a No. 1 feeding bin, a No. 2 feeding bin, a No. 3 feeding bin and a liquid material tank; the multi-chamber continuous kneading machine comprises a discharge port, a first feeding port, a second feeding port and a third feeding port.

[0012] The discharge end of the No. 1 feeding bin is connected to the feed end of the screw feeder, the discharge end of the screw feeder is connected to the feed end of the first feeding port, and the discharge end of the first feeding port is connected to the first chamber of the multi-chamber continuous kneading machine; the discharge end of the No. 2 feeding bin is connected to the feed end of the No. 1 vibrating feeder, the discharge end of the No. 1 vibrating feeder is connected to the feed end of the second feeding port, and the discharge end of the second feeding port is connected to the second chamber of the multi-chamber continuous kneading machine; the discharge end of the No. 3 feeding bin is connected to the feed end of the No. 2 vibrating feeder, the discharge end of the No. 2 vibrating feeder is connected to the feed end of the third feeding port, and the discharge end of the third feeding port is connected to the third chamber of the multi-chamber continuous kneading machine.

[0013] The discharge end of the liquid material tank is connected to the feed ends of liquid feeder No. 1 and liquid feeder No. 2, the discharge end of liquid feeder No. 1 is connected to the first feeding port, and the discharge end of liquid feeder No. 2 is connected to the third feeding port; a waste tray is provided at the end of the discharge port of the multi-chamber continuous kneading machine.

[0014] Specifically, the method comprises the following steps:

[0015] Step 1: Mixing of explosives and fire:

[0016] The raw materials required for the explosive mixing operation stored in the No. 1 feeding bin, the No. 2 feeding bin, the No. 3 feeding bin and the liquid material tank are added into the chamber of the multi-chamber continuous kneading machine through the first feeding port, the second feeding port and the third feeding port respectively for mixing.

[0017] Step 2: Perform security cleanup:

[0018] Step 2.1, switching the discharge port of the multi-chamber continuous kneading machine from the pouring station to the waste collection station, and collecting the waste with a waste tray.

[0019] Step 2.2, continue to add, mix and discharge materials until the remaining explosive and explosive energetic components in the No. 2 feeding bin and the No. 3 feeding bin are completely added into the multi-chamber continuous kneading machine.

[0020] Step 2.3, turn off the No. 1 liquid feeder, No. 2 liquid feeder, screw feeder, No. 1 vibrating feeder, No. 2 vibrating feeder and multi-chamber continuous kneading machine, and add the non-energetic powder material into the No. 2 feeding bin and the No. 3 feeding bin as substitute materials.

[0021] Step 2.4, start liquid feeder No. 1 and liquid feeder No. 2, start the multi-chamber continuous kneading machine after 2 minutes, start the screw feeder, vibrating feeder No. 1 and vibrating feeder No. 2 after the paddle speed stabilizes, and restart continuous feeding, mixing and discharging.

[0022] Step 2.5, after the non-energetic powder materials in No. 2 feeding bin, No. 3 feeding bin, No. 1 vibrating feeder and No. 2 vibrating feeder are consumed, close all feeders and stop feeding, continue to keep the multi-chamber continuous kneading machine open, until there is no obvious slurry flowing out of the discharge port, and then close the multi-chamber continuous kneading machine.

[0023] Step 2.6, open the front cover of the multi-chamber continuous kneading machine to expose the internal chamber and paddles. The personnel enter the site and use a copper shovel to scrape off the residual slurry adhering to the inner wall of the chamber and the paddles and wipe them with ethyl acetate. The residual slurry is collected in a waste barrel, and then a high-pressure air gun is used to blow the inside of the No. 2 and No. 3 feeding bins to remove the residual non-energetic powder materials for the next operation. The cleaning process is now completed.

[0024] Step 3. After the safety cleanup is completed, repeat step 1 to carry out the next pyrotechnics and explosives mixing operation.

[0025] Specifically, in step 2.3, the mass ratio of the non-energetic powder material added to the No. 2 feeding bin and the No. 3 feeding bin is (30-60): (30-60).

[0026] Specifically, the feeding speed of each feeder in step 2.4 is consistent with the feeding speed of each corresponding feeder in step 1.

[0027] Specifically and optionally, in step one, the raw materials required for the explosive mixing operation include aluminum powder, hexachlorobenzene, ammonium perchlorate and terminal hydroxyl polybutadiene; wherein hexachlorobenzene and ammonium perchlorate are energetic components of the explosive, aluminum powder is a non-energetic component of the explosive, and terminal hydroxyl polybutadiene is a liquid component of the explosive.

[0028] Specifically and optionally, in step one, the raw materials required for the explosive mixing operation include aluminum powder, octogenin, ammonium perchlorate and terminal hydroxyl polybutadiene; wherein octogenin and ammonium perchlorate are energetic components of the explosive, aluminum powder is a non-energetic component of the explosive, and terminal hydroxyl polybutadiene is a liquid component of the explosive.

[0029] Specifically, the non-energetic components of the explosive are fed by a screw feeder, and the energetic components of the explosive are fed by a vibrating feeder.

[0030] Specifically, the step 1 includes the following steps:

[0031] Step 1.1, pre-store aluminum powder, hexachlorobenzene and ammonium perchlorate in No. 1 feeding bin, No. 2 feeding bin and No. 3 feeding bin respectively; or pre-store aluminum powder, octogenin and ammonium perchlorate in No. 1 feeding bin, No. 2 feeding bin and No. 3 feeding bin respectively; pre-store liquid terminal hydroxyl polybutadiene in a liquid tank.

[0032] Step 1.2, start the No. 1 liquid feeder and the No. 2 liquid feeder, and add the hydroxy-terminated polybutadiene into the first chamber and the third chamber of the multi-chamber continuous kneader through the first feeding port and the third feeding port respectively.

[0033] Step 1.3, start the multi-chamber continuous kneader after 2 minutes, start the screw feeder, the first vibrating feeder and the second vibrating feeder after the blade speed stabilizes, and add aluminum powder, hexachlorobenzene and ammonium perchlorate into the first chamber, the second chamber and the third chamber of the multi-chamber continuous kneader through the first feeding port, the second feeding port and the third feeding port respectively, and start continuous mixing and discharging.

[0034] Specifically, in step 1.2, the volume ratio of the hydroxy-terminated polybutadiene entering the first chamber and the third chamber of the multi-chamber continuous kneader is 7:3.

[0035] Specifically, in step 1.3, the residence time of the material in the chamber during mixing is 25 to 35 minutes, and the blade speed of the multi-chamber continuous kneader during mixing is 30 to 60 rpm.

[0036] Specifically, the mass ratio of the added amount of the non-energetic powder material to the mass ratio of the energetic components of the explosive is (15-40):(50-75).

[0037] The beneficial technical effects of the present invention compared with the prior art are as follows: the present invention uses non-energetic powder materials as substitute materials to extrude a large amount of energetic components of explosives that have not reached a completely mixed state remaining in the chamber, so that only a small amount of materials adhering to the blades and the chamber wall remain in the mixing device, and at this time, the content of energetic components of explosives in the residual materials is significantly lower than that of the mixed materials before the substitute materials are extruded, and the remaining non-energetic powder materials are not dangerous, so the mixing equipment can be directly opened to remove them. The present invention greatly reduces the danger in the manual cleaning process, avoids the occurrence of safety accidents, protects the lives and property of personnel, and meets the current demand for safe supply of explosives production. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] Figure 1 This is a schematic diagram of the overall structure of the continuous mixing equipment for explosives and gunpowder.

[0039] The meanings of the numbers in the figure are: 1-multi-chamber continuous kneading machine, 2-No. 1 feeding bin, 3-No. 2 feeding bin, 4-No. 3 feeding bin, 5-liquid tank, 6-screw feeder, 7-No. 1 vibration feeder, 8-No. 2 vibration feeder, 9-No. 1 liquid feeder, 10-No. 2 liquid feeder, 11-waste tray-.

[0040] 101 - first feeding port, 102 - second feeding port, 103 - third feeding port, 104 - discharge port.

[0041] The technical solution of the present invention is further described below in conjunction with embodiments. DETAILED DESCRIPTION

[0042] In the present invention, the multi-chamber continuous kneading machine 1 adopts a multi-chamber continuous kneading machine known in the prior art, which is recorded in the Chinese patent application number CN202011202790.3.

[0043] It should be noted that all raw materials used in the present invention, unless otherwise specified, are raw materials known in the art.

[0044] In accordance with the above technical scheme, specific embodiments of the present invention are given below. It should be noted that the present invention is not limited to the following specific embodiments, and all equivalent changes made on the basis of the technical scheme of this application fall within the protection scope of the present invention.

[0045] Embodiment 1:

[0046] This embodiment provides a continuous mixing device for explosives and explosives, such as Figure 1As shown, it includes a multi-chamber continuous kneading machine 1, a No. 1 feeding bin 2, a No. 2 feeding bin 3, a No. 3 feeding bin 4 and a liquid material tank 5; the multi-chamber continuous kneading machine 1 includes a discharge port 104, a first feeding port 101, a second feeding port 102 and a third feeding port 103.

[0047] The discharge end of the No. 1 feeding bin 2 is connected to the feed end of the screw feeder 6, the discharge end of the screw feeder 6 is connected to the feed end of the first feeding port 101, and the discharge end of the first feeding port 101 is connected to the first chamber of the multi-chamber continuous kneading machine 1; the discharge end of the No. 2 feeding bin 3 is connected to the feed end of the No. 1 vibrating feeder 7, the discharge end of the No. 1 vibrating feeder 7 is connected to the feed end of the second feeding port 102, and the discharge end of the second feeding port 102 is connected to the second chamber of the multi-chamber continuous kneading machine 1; the discharge end of the No. 3 feeding bin 4 is connected to the feed end of the No. 2 vibrating feeder 8, the discharge end of the No. 2 vibrating feeder 8 is connected to the feed end of the third feeding port 103, and the discharge end of the third feeding port 103 is connected to the third chamber of the multi-chamber continuous kneading machine 1.

[0048] The discharge end of the liquid material tank 5 is connected to the feed ends of the No. 1 liquid feeder 9 and the No. 2 liquid feeder 10, the discharge end of the No. 1 liquid feeder 9 is connected to the first feeding port 101, and the discharge end of the No. 2 liquid feeder 10 is connected to the third feeding port 103; a waste tray 11 is provided at the end of the discharge port 104 of the multi-chamber continuous kneading machine 1.

[0049] Embodiment 2:

[0050] This embodiment provides a method for safe production of continuous mixing of explosives and propellants, which comprises: after a mixing operation of explosives and propellants is completed, a non-energetic powder material is used as a substitute material to safely clean up the energetic components of the explosives and propellants remaining in the continuous mixing equipment of explosives and propellants, and then the next mixing operation of explosives and propellants is carried out; this method is implemented based on the continuous mixing equipment of explosives and propellants in Example 1.

[0051] In this embodiment, the raw materials required for the explosive mixing operation include aluminum powder, hexachlorobenzene, ammonium perchlorate and HTPB (hydroxyl-terminated polybutadiene). The solid phase (i.e., aluminum powder, hexachlorobenzene and ammonium perchlorate) content in the explosive mixture is 88%, wherein the aluminum powder is a non-energetic component of the explosive, the hydroxyl-terminated polybutadiene is a liquid component of the explosive, hexachlorobenzene and ammonium perchlorate are energetic components of the explosive, and the substitute materials are all anhydrous sodium sulfate.

[0052] The method specifically comprises the following steps:

[0053] Step 1: Mixing of explosives and fire:

[0054] Step 1.1, pre-store aluminum powder, hexachlorobenzene and ammonium perchlorate in No. 1 feeding bin 2, No. 2 feeding bin 3 and No. 3 feeding bin 4 respectively, and pre-store the HTPB of liquid material in the liquid material tank 5.

[0055] Step 1.2, start liquid feeder No. 1 9 and liquid feeder No. 2 10, and add HTPB into the first chamber and the third chamber of the multi-chamber continuous kneading machine 1 through the first feeding port 101 and the third feeding port 103 respectively, and the volume ratio of HTPB entering the first chamber and the third chamber is 7:3; the feeding speed of liquid feeder No. 1 9 is 16.8 kg / h, and the feeding speed of liquid feeder No. 2 10 is 7.2 kg / h.

[0056] Step 1.3, after 2 minutes, start the multi-chamber continuous kneading machine 1, wait for the blade speed to stabilize, start the screw feeder 6, the first vibrating feeder 7 and the second vibrating feeder 8, respectively add aluminum powder, hexachlorobenzene and ammonium perchlorate into the first chamber, the second chamber and the third chamber of the multi-chamber continuous kneading machine 1 through the first feeding port 101, the second feeding port 102 and the third feeding port 103, start mixing and discharging, the residence time of the material in the chamber during mixing is about 30 minutes, and the mixing and discharging capacity of the multi-chamber continuous kneading machine 1 is 200kg / h. Among them, the non-energetic component powder (aluminum powder) of the explosive is fed by a screw feeder, and the energetic components of the explosive (hexachlorobenzene and ammonium perchlorate) are fed by a vibrating feeder.

[0057] Step 2: Perform security cleanup:

[0058] Step 2.1, switching the discharge port 104 of the multi-chamber continuous kneading machine 1 from the pouring station to the waste collection station, and using the waste tray 11 to collect the waste.

[0059] Step 2.2, continue to add, mix and discharge until the small amount of RDX and ammonium perchlorate remaining in No. 2 feeding bin 3, No. 3 feeding bin 4, No. 1 liquid feeder 9 and No. 2 liquid feeder 10 are completely added to the multi-chamber continuous kneading machine 1.

[0060] Step 2.3, turn off all feeders and multi-chamber continuous kneading machine 1, and personnel enter the site to add 41 kg of anhydrous sodium sulfate to No. 2 feeding silo 3, and add 45 kg of anhydrous sodium sulfate to No. 3 feeding silo 4, as substitutes for RDX and ammonium perchlorate, respectively.

[0061] For liquid materials and non-energetic powder materials in the product formula, the amount required in step 2.4 can be added to the liquid material tank and the feeding bin when the current shift is first fed. In addition, it can also be added when the substitute material is fed. In this embodiment, since sufficient amounts of HTPB and aluminum powder have been added to the liquid material tank 5 and the No. 1 feeding bin 2 respectively when the current shift is first fed, and the remaining materials can continue to be used for the next shift production, there is no need to feed them a second time, and only anhydrous sodium sulfate needs to be added.

[0062] In this embodiment, the amount of anhydrous sodium sulfate added can meet the demand for continuous feeding for 40 minutes. The amount of anhydrous sodium sulfate added should ensure that the continuous feeding time is not less than the residence time of the material in the chamber, so that the energetic waste can be squeezed out or diluted as much as possible, thereby minimizing the danger of the cleaning process.

[0063] Step 2.4, personnel evacuate to the explosion-proof control room outside the site, start liquid feeder No. 1 9 and liquid feeder No. 2 10, start the multi-chamber continuous kneading machine 1 after 2 minutes, start the screw feeder 6, vibrating feeder No. 1 7 and vibrating feeder No. 2 8 after the paddle speed stabilizes, and restart continuous feeding, mixing and discharging. The feeding speed of all feeders should be consistent with the feeding speed during normal mixing and pouring operations.

[0064] Step 2.5, after the anhydrous sodium sulfate in No. 2 feeding bin 3, No. 3 feeding bin 4, No. 1 vibrating feeder 7 and No. 2 vibrating feeder 8 is consumed, close all feeders and stop feeding, and keep the multi-chamber continuous kneading machine 1 open until there is no obvious slurry flowing out of the discharge port 104, and then close the multi-chamber continuous kneading machine 1.

[0065] Step 2.6, through remote operation, the front cover of the multi-chamber continuous kneading machine 1 is opened by a hydraulic cylinder to expose the internal chamber and the blades. The personnel enter the site, use a copper shovel to scrape off the residual slurry adhering to the inner wall of the chamber and the blades and wipe and clean them with ethyl acetate, collect the residual slurry into a waste bucket, and then use a high-pressure air gun to purge the inside of the No. 2 feeding bin 3 and the No. 3 feeding bin 4 to remove the residual anhydrous sodium sulfate for the next operation, thus completing the cleaning process. In this embodiment, the handle of the copper shovel used is grounded to promptly conduct away the generated static electricity.

[0066] In this embodiment, the opening and closing of the feeding and mixing equipment are all achieved through remote control. Except for the anhydrous sodium sulfate feeding and manual cleaning operations, all other on-site unmanned operations are achieved.

[0067] Step 3. After the safety cleanup is complete, repeat step 1 to mix the explosives for the next shift.

[0068] In this embodiment, in step one and step two, the liquid feeder 10 is first turned on, then the multi-chamber continuous kneading machine 1 is turned on, and finally the screw feeder 6, the first vibrating feeder 7 and the second vibrating feeder 8 are turned on. Such operation can improve the wettability of the powder material and ensure that the slurry has good fluidity.

[0069] Embodiment 3:

[0070] This embodiment provides a method for safe production of continuous mixing of explosives and propellants, which is implemented based on the continuous mixing equipment for explosives and propellants in embodiment 1. The method is basically the same as embodiment 2, except that anhydrous potassium sulfate is used as a substitute.

[0071] Embodiment 4:

[0072] This embodiment provides a method for safe production of continuous mixing of explosives and propellants, which is implemented based on the continuous mixing equipment of explosives and propellants in embodiment 1. The method is basically the same as embodiment 2, except that anhydrous calcium carbonate is used as a substitute.

[0073] Embodiment 5:

[0074] This embodiment provides a method for safe production of continuous mixing of explosives, which is implemented based on the continuous mixing equipment of explosives in embodiment 1. This method is basically the same as embodiment 2, except that: in this embodiment, the raw materials required for the mixing of explosives include aluminum powder, octogenin, ammonium perchlorate and HTPB (hydroxyl-terminated polybutadiene). The solid phase (i.e., aluminum powder, octogenin and ammonium perchlorate) in the explosive mixture is 88%, wherein aluminum powder is a non-energetic component of explosives, hydroxyl-terminated polybutadiene is a liquid component of explosives, octogenin and ammonium perchlorate are energetic components of explosives, and their substitutes are all anhydrous sodium sulfate.

[0075] In this embodiment, step one specifically includes the following steps:

[0076] Step 1.1, pre-store aluminum powder, octogenin and ammonium perchlorate in No. 1 feeding bin 2, No. 2 feeding bin 3 and No. 3 feeding bin 4 respectively, and pre-store the HTPB of liquid material in the liquid material tank 5.

[0077] Step 1.2, start liquid feeder No. 1 9 and liquid feeder No. 2 10, and add HTPB into the first chamber and the third chamber of the multi-chamber continuous kneading machine 1 through the first feeding port 101 and the third feeding port 103 respectively, and the volume ratio of HTPB entering the first chamber and the third chamber is 7:3; the feeding speed of liquid feeder No. 1 9 is 16.8 kg / h, and the feeding speed of liquid feeder No. 2 10 is 7.2 kg / h.

[0078] Step 1.3, after 2 minutes, start the multi-chamber continuous kneading machine 1, wait for the blade speed to stabilize, start the screw feeder 6, the first vibrating feeder 7 and the second vibrating feeder 8, respectively, add aluminum powder, octochrome and ammonium perchlorate to the first chamber, the second chamber and the third chamber of the multi-chamber continuous kneading machine 1 through the first feeding port 101, the second feeding port 102 and the third feeding port 103, and start mixing and discharging. During mixing, the residence time of the material in the chamber is about 30 minutes, and the mixing and discharging capacity of the multi-chamber continuous kneading machine 1 is 200kg / h. Among them, the non-energetic component powder (aluminum powder) of the explosive is fed by a screw feeder, and the energetic components of the explosive (octochrome, ammonium perchlorate) are fed by a vibrating feeder.

[0079] Embodiment 6:

[0080] This embodiment provides a method for safe production of continuous mixing of explosives and propellants, which is implemented based on the continuous mixing equipment for explosives and propellants of embodiment 1. The method is basically the same as embodiment 5, except that anhydrous potassium sulfate is used as a substitute to safely clean the continuous mixing equipment for explosives and propellants.

[0081] Embodiment 7:

[0082] This embodiment provides a method for safe production of continuous mixing of explosives and propellants, which is implemented based on the continuous mixing equipment of explosives and propellants in embodiment 1. The method is basically the same as embodiment 5, except that anhydrous calcium carbonate is used as a substitute to safely clean the continuous mixing equipment of explosives and propellants.

Claims

1. A method for safe production of continuous mixing of explosives and propellants, characterized in that: The method comprises: after a pyrotechnics mixing operation is completed, a non-energetic powder material is used as a substitute material to safely clean up the pyrotechnics energetic components remaining in the pyrotechnics continuous mixing equipment, and then the next pyrotechnics mixing operation is carried out; The non-energetic powder material is selected from one or more of anhydrous sodium sulfate, anhydrous potassium sulfate, and anhydrous calcium carbonate; The energetic components of the explosive are selected from one or more of RDX, ammonium perchlorate and octogenin.

2. The method for safe production of continuous mixing of explosives and propellants as claimed in claim 1, characterized in that: The explosive continuous mixing device comprises a multi-chamber continuous kneading machine (1), a No. 1 feeding bin (2), a No. 2 feeding bin (3), a No. 3 feeding bin (4) and a liquid material tank (5); the multi-chamber continuous kneading machine (1) comprises a discharge port (104), a first feeding port (101), a second feeding port (102) and a third feeding port (103); The discharge end of the No. 1 feeding bin (2) is connected to the feed end of the screw feeder (6), the discharge end of the screw feeder (6) is connected to the feed end of the first feeding port (101), the discharge end of the first feeding port (101) is connected to the first chamber of the multi-chamber continuous kneading machine (1); the discharge end of the No. 2 feeding bin (3) is connected to the feed end of the No. 1 vibrating feeder (7), the discharge end of the No. 1 vibrating feeder (7) is connected to the feed end of the second feeding port (101). The feeding end of the No. 3 feeding port (102) is connected to the feeding end of the No. 2 vibrating feeder (8), the discharging end of the No. 2 vibrating feeder (8) is connected to the feeding end of the third feeding port (103), and the discharging end of the third feeding port (103) is connected to the third chamber of the multi-chamber continuous kneading machine (1); the discharging end of the No. 3 feeding bin (4) is connected to the feeding end of the No. 2 vibrating feeder (8), the discharging end of the No. 2 vibrating feeder (8) is connected to the feeding end of the third feeding port (103), and the discharging end of the third feeding port (103) is connected to the third chamber of the multi-chamber continuous kneading machine (1); The discharge end of the liquid material tank (5) is connected to the feed ends of the first liquid feeder (9) and the second liquid feeder (10), the discharge end of the first liquid feeder (9) is connected to the first feed port (101), and the discharge end of the second liquid feeder (10) is connected to the third feed port (103); a waste tray (11) is provided at the end of the discharge port (104) of the multi-chamber continuous kneading machine (1); The method specifically comprises the following steps: Step 1: Mixing of explosives and fire: The raw materials required for the explosive mixing operation stored in the No. 1 feeding bin (2), the No. 2 feeding bin (3), the No. 3 feeding bin (4) and the liquid material tank (5) are added into the chamber of the multi-chamber continuous kneading machine (1) through the first feeding port (101), the second feeding port (102) and the third feeding port (103) for mixing; Step 2: Perform security cleanup: Step 2.1, switching the discharge port (104) of the multi-chamber continuous kneading machine (1) from the pouring station to the waste collection station, and using the waste tray (11) to collect the waste; Step 2.2, continue to add, mix and discharge materials until the remaining explosive and explosive energetic components in the No. 2 feeding bin (3) and the No. 3 feeding bin (4) are completely added into the multi-chamber continuous kneading machine (1); Step 2.3, turn off the No. 1 liquid feeder (9), the No. 2 liquid feeder (10), the screw feeder (6), the No. 1 vibrating feeder (7), the No. 2 vibrating feeder (8) and the multi-chamber continuous kneading machine (1), and add the non-energetic powder material into the No. 2 feeding bin (3) and the No. 3 feeding bin (4) as substitute material; Step 2.4, start the No. 1 liquid feeder (9) and the No. 2 liquid feeder (10), start the multi-chamber continuous kneader (1) after 2 minutes, and start the screw feeder (6), the No. 1 vibrating feeder (7) and the No. 2 vibrating feeder (8) after the blade speed stabilizes, and restart the continuous feeding, mixing and discharging; Step 2.5, after the non-energetic powder materials in the No. 2 feeding bin (3), the No. 3 feeding bin (4), the No. 1 vibrating feeder (7) and the No. 2 vibrating feeder (8) are completely consumed, all the feeders are closed to stop feeding, and the multi-chamber continuous kneading machine (1) is kept open until there is no obvious slurry flowing out of the discharge port (104), and the multi-chamber continuous kneading machine (1) is closed; Step 2.6, open the front cover of the multi-chamber continuous kneading machine (1) to expose the internal chamber and the blades, and personnel enter the site, use a copper shovel to scrape off the residual slurry adhering to the inner wall of the chamber and the blades and wipe and clean them with ethyl acetate, collect the residual slurry into a waste barrel, and then use a high-pressure air gun to blow the inside of the No. 2 feeding bin (3) and the No. 3 feeding bin (4) to remove the residual non-energetic powder material for the next operation, and the cleaning process is completed; Step 3: After the safety cleanup is completed, repeat step 1 to carry out the next pyrotechnics and explosives mixing operation.

3. The method for safe production of continuous mixing of explosives and propellants as claimed in claim 2, characterized in that: In step 2.3, the mass ratio of the non-energetic powder material added to the No. 2 feeding bin (3) and the No. 3 feeding bin (4) is (30-60): (30-60).

4. The method for safe production of continuous mixing of explosives and propellants as claimed in claim 2, characterized in that: The feeding speed of each feeder in step 2.4 is consistent with the feeding speed of each corresponding feeder in step 1.

5. The method for safe production of continuous mixing of explosives and propellants as claimed in claim 2, characterized in that: In step 1, the raw materials required for the explosive mixing operation include aluminum powder, hexachlorobenzene, ammonium perchlorate and terminal hydroxyl polybutadiene; wherein hexachlorobenzene and ammonium perchlorate are energetic components of the explosive, aluminum powder is a non-energetic component of the explosive, and terminal hydroxyl polybutadiene is a liquid component of the explosive; The raw materials required for the mixing operation of explosives and pyrotechnics include aluminum powder, octogenin, ammonium perchlorate and terminal hydroxyl polybutadiene; among them, octogenin and ammonium perchlorate are energetic components of explosives and pyrotechnics, aluminum powder is a non-energetic component of explosives and pyrotechnics, and terminal hydroxyl polybutadiene is a liquid component of explosives and pyrotechnics.

6. The method for safe production of continuous mixing of explosives and propellants as claimed in claim 5, characterized in that: The non-energetic components of the explosive are fed by a screw feeder, and the energetic components of the explosive are fed by a vibrating feeder.

7. The method for safe production of continuous mixing of explosives and propellants as claimed in claim 5, characterized in that: The step 1 specifically includes the following steps: Step 1.1, pre-store aluminum powder, hexachlorobenzene and ammonium perchlorate in No. 1 feeding bin (2), No. 2 feeding bin (3) and No. 3 feeding bin (4), respectively; or pre-store aluminum powder, octogenin and ammonium perchlorate in No. 1 feeding bin (2), No. 2 feeding bin (3) and No. 3 feeding bin (4), respectively; pre-store liquid hydroxyl-terminated polybutadiene in a liquid tank (5); Step 1.2, start the first liquid feeder (9) and the second liquid feeder (10), and add the hydroxy-terminated polybutadiene into the first chamber and the third chamber of the multi-chamber continuous kneader (1) through the first feeding port (101) and the third feeding port (103), respectively; Step 1.3, after 2 minutes, start the multi-chamber continuous kneading machine (1), and after the blade speed stabilizes, start the screw feeder (6), the first vibrating feeder (7) and the second vibrating feeder (8), and add aluminum powder, hexachlorobenzene and ammonium perchlorate into the first chamber, the second chamber and the third chamber of the multi-chamber continuous kneading machine (1) through the first feeding port (101), the second feeding port (102) and the third feeding port (103), respectively, to start continuous mixing and discharging.

8. The method for safe production of continuous mixing of explosives and propellants as claimed in claim 7, characterized in that: In step 1.2, the volume ratio of the hydroxy-terminated polybutadiene entering the first chamber and the third chamber of the multi-chamber continuous kneader (1) is 7:

3.

9. The method for safe production of continuous mixing of explosives and propellants as claimed in claim 7, characterized in that: In step 1.3, the residence time of the materials in the chamber during mixing is 25 to 35 minutes, and the blade speed of the multi-chamber continuous kneading machine (1) during mixing is 30 to 60 rpm.

10. The method for safe production of continuous mixing of explosives and propellants as claimed in claim 1, characterized in that: The mass ratio of the added amount of non-energetic powder material to the mass ratio of the energetic components of the explosive is (15-40):(50-75).

Citation Information

Patent Citations

  • Environment-friendly cleaning agent for mechanical equipment

    CN103436394A

  • Preparation method for calcium carbonate for screw cleaning agent

    CN106978277A

  • Inert demoulding material

    CN111454486A

  • Energetic material kneading device and method

    CN112266310A

  • Cleaning material and method for cleaning high-burning-rate solid propellant adhered in mixing equipment

    CN114213199A