Non-fluoropolymer and surface treating agent

By copolymerizing silicone-containing acrylate monomers with long-chain alkyl acrylate monomers, a non-fluorinated copolymer was prepared, which solved the environmental pollution problem of fluorinated waterproofing agents and the poor affinity problem of organosilicon waterproofing agents, and achieved a durable and stable hydrophobic and oleophobic effect on the fiber surface.

CN118909187AInactive Publication Date: 2024-11-08DYMATIC CHEM +2

Patent Information

Application Number
CN202410957088.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-16
Publication Date
2024-11-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing fluorinated waterproofing agents generate recalcitrant organic pollutants during the production process, which are harmful to the environment and health. Furthermore, traditional silicone waterproofing agents have poor affinity with fibers, poor dynamic water repellency, and unstable water/oil repellency properties.

Method used

Non-fluorinated copolymers are prepared by copolymerizing silicone-containing acrylate monomers with long-chain alkyl acrylate monomers. The synergistic effect between polar side groups and long-chain alkyl groups is utilized to inhibit surface reconstruction and improve water/oil repellency.

Benefits of technology

The prepared non-fluorinated copolymer forms a durable and stable low surface energy film on the fiber surface, giving the fiber excellent hydrophobic and oleophobic properties, making it environmentally friendly and stable.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004949172950000021
    Figure BDA0004949172950000021
  • Figure BDA0004949172950000022
    Figure BDA0004949172950000022
  • Figure BDA0004949172950000023
    Figure BDA0004949172950000023
Patent Text Reader

Abstract

The invention provides a non-fluorine polymer and a surface treating agent containing the same. The non-fluorine polymer comprises the following components in percentage by mass: 10-40% of a non-fluorine copolymer; 2%-8% of a surfactant; 2%-10% of a component agent; and the balance of deionized water. The non-fluorine copolymer is obtained by polymerizing a silicon-containing acrylate monomer (a), an acrylate monomer (b) having a C1-30 saturated hydrocarbon group or cyclic hydrocarbon group, and a functional monomer (c) in the presence of a chain transfer agent and a polymerization initiator. The non-fluorine copolymer prepared on the basis of the silicon-containing acrylate monomer or the surface treating agent containing the non-fluorine copolymer imparts excellent water repellency and stain resistance to base materials such as fibers.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of dyeing and finishing auxiliaries, in particular to a non-fluorine polymer and a surface treatment agent containing the polymer. Background Art

[0002] With the rise of outdoor sports and people's emphasis on health and safety protection, the market demand for water-repellent textiles is growing, and the scale of related industries exceeds 100 billion yuan. At present, the waterproofing agents used in the market are mainly fluorine-based waterproofing agents, but these high-performance fluorinated derivatives inevitably bring about perfluorooctanoic acid (PFOA) or perfluorooctane sulfonic acid (PFOS) residues during the production process. They are one of the most difficult to degrade organic pollutants found in the world. They are bioaccumulative and have long-range migration properties. They are difficult to continue to degrade in the natural environment, and they are very harmful to human health and the living environment. As early as 2012, the Stockholm Convention on Persistent Organic Pollutants had included PFOA and PFOS in the list of chemicals to be banned, and a comprehensive ban has become a general trend. Today, when the concept of ecological protection is becoming increasingly popular, fluorine-free waterproofing agents are more easily accepted by consumers, so the development of fluorine-free waterproofing agents has become a new research hotspot.

[0003] After high-temperature baking, silicone waterproofing agents can form a layer of low surface tension water-repellent film on the fiber surface. The hydrophobic -CH3 on the film surface stretches outward, like small umbrellas arranged on the fiber surface, giving the substrate good water-repellent, oil-repellent, and dirt-repellent functions after finishing. However, traditional silicones have poor affinity with fibers, and the silicon-containing chain segments are highly mobile. When their surfaces come into contact with polar liquids such as water, surface reconstruction occurs, the dynamic water repellency is poor, and the water / oil repellency is significantly reduced, and a long-lasting stable low surface energy cannot be obtained. Therefore, in order to solve this problem, a fluorine-free waterproofing agent is prepared by copolymerizing a silicon-containing acrylate monomer with a long-chain alkyl acrylate monomer. The synergistic effect between the polar side groups and the long-chain alkyl groups in the copolymer structure affects the activity of the silicon-containing side groups, which is beneficial to inhibiting surface reconstruction and improving the water / oil repellency of the fluorine-free waterproofing agent. Summary of the invention

[0004] The purpose of the present invention is to provide a non-fluorine polymer and a surface treatment agent containing the polymer, which can impart excellent hydrophobicity and oleophobicity to substrates such as fibers, and is green, environmentally friendly, and harmless to human health, thereby overcoming the shortcomings of the prior art.

[0005] In order to solve the above technical problems, the present invention is achieved through the following technical solutions: a non-fluorine polymer and a treating agent containing the polymer, comprising the following components by mass percentage:

[0006] 10% to 40% of a non-fluorine copolymer; 2% to 8% of a surfactant; 2% to 10% of a component; and the balance is deionized water; the non-fluorine copolymer is obtained by polymerizing a silicon-containing acrylate monomer (a), an acrylate monomer having a saturated hydrocarbon group or a cyclic hydrocarbon group with 1 to 30 carbon atoms (b), and a functional monomer (c) in the presence of a chain transfer agent and a polymerization initiator.

[0007] The silicon-containing acrylate monomer (a) is a silicon-containing acrylate or a derivative thereof, and its general structural formula is:

[0008]

[0009] wherein X1, X2 and X3 are H, CH3, Cl or Br; Y1 is a chemical single bond or one or more of -NH-, -NR2-, -NH-CO-, -NR2-CO-, -NHCONH-, -NHCOO-, -NH-SO2-, -NR2-SO2-; n1 is an integer from 1 to 20;

[0010] The structural formulas of Z1, Z2 and Z3 are:

[0011]

[0012] In the formula, A is a chemical single bond or an oxygen atom, R1, R2 and R3 are saturated hydrocarbon groups or cyclic hydrocarbon groups having 1 to 30 carbon atoms; and m is an integer of 0 to 300.

[0013] The silicon-containing acrylate monomer (a) may be one substance or a mixture of multiple substances conforming to the general formula.

[0014] The structural formula of the acrylic acid ester monomer (b) having a saturated hydrocarbon group or a cyclic hydrocarbon group having 1 to 30 carbon atoms is:

[0015]

[0016] In the formula, X4, X5 and X6 are H, CH3, Cl or Br; R4 represents a saturated hydrocarbon group or a cyclic hydrocarbon group having 1 to 30 carbon atoms; Y2 is a chemical single bond or one or more of -NH-, -NR5-, -NH-CO-, -NR5-CO-, -NHCONH-, -NHCOO-, -NH-SO2-, -NR5-SO2-, R5 is an alkyl group having 1 to 4 carbon atoms; n2 is an integer from 1 to 20; it can be a substance or a mixture of multiple substances that conform to the general formula.

[0017] The functional monomer (c) is selected from one or more of glycidyl (meth)acrylate, acrylamide, diacetone acrylamide combined with adipic dihydrazide system, ethylene glycol dimethacrylate, trimethylolpropane tri(meth)acrylate, divinylbenzene, dimethylaminoethyl (meth)acrylate, (methoxy)polyethylene glycol (meth)acrylate, (meth)acryloyloxyethyl trimethylammonium chloride, N-acryl pyrrolidone, 3-chloro-2-hydroxy-propyl methacrylate, hydroxyethyl (meth)acrylate, hydroxymethyl (meth)acrylate, organic silicone resin containing reactive groups, vinyl chloride, vinylidene chloride, butadiene, isoprene, and chloroprene.

[0018] The reactive group-containing organic silicone resin is one or more of MQ resin, MT resin, MDT resin or caged polysilsesquioxane (POSS) containing reactive groups, and the reactive groups are one of (meth)acryloyloxy, (meth)acrylamide, vinyl or mercapto.

[0019] The chain transfer agent is alkyl mercaptan.

[0020] The polymerization initiator is an azo-based, peroxide-based, or redox-based polymerization initiator.

[0021] The surfactant contains one or more of a cationic surfactant and a nonionic surfactant.

[0022] The cationic surfactant is one or more of amine, amine salt, quaternary ammonium salt, imidazoline and imidazolinium salt.

[0023] The nonionic surfactant is one or more of ether, ester, ester ether, alkanolamide, polyol and amine oxide;

[0024] The auxiliary agents include pH adjusting auxiliary agents and organic solvents.

[0025] The pH adjusting auxiliary agent includes acid, alkali or amino acid, and makes the pH value of the treating agent be between 2 and 9.

[0026] The organic solvent is selected from one or a mixture of two of dipropylene glycol, tripropylene glycol, dipropylene glycol ethyl ether, tripropylene glycol ethyl ether, acetone, methyl ethyl ketone, ethyl acetate, n-propyl acetate, butyl acetate, N-methyl-2-pyrrolidone, N,N-dimethylformamide, isopropanol, and n-propanol.

[0027] The present invention has the following beneficial effects:

[0028] The present invention is based on the copolymerization of silicon-containing acrylate monomers and long-chain alkyl acrylate monomers to prepare a fluorine-free waterproofing agent. The synergistic effect between the polar side groups and the long-chain alkyl groups in the copolymer structure affects the activity of the silicon-containing side groups, which is beneficial to inhibiting the silicon-containing side groups enriched on the outermost surface from returning to the polymer body, thereby giving substrates such as fibers a long-lasting, stable and low surface energy. In addition, the polymer of the present invention avoids the use of fluorine-containing acrylate monomers, is environmentally friendly, and has high commercial value. DETAILED DESCRIPTION

[0029] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0030] In order to verify the water repellency and stain resistance of the textile treated with the fluorine-free water repellent of the present invention, a standard method can be used for inspection for comparison. The standard method is to use the national standard GB 4745-2012 to inspect the water repellency and the national standard GB 30159.1-2013 to inspect the stain resistance. The following is a brief introduction to the method.

[0031] (1) Water repellent effect

[0032] National standard GB 4745-2012 test method. Cut 18×18cm finished fabric and stretch it on the clamp and place it at an angle of 45°. Set a nozzle 150mm above it and quickly sprinkle 250ml of water on the inclined fabric within 25-30s. After the spraying is completed, take out the clamp and knock it horizontally twice from the front downward to observe the experimental wetting degree, then use text description and compare with the standard picture to evaluate its level, and take the average of the two times.

[0033] The rating standards are shown in Table 1.

[0034] Table 1

[0035]

[0036] (2) Stain resistance

[0037] National standard GB 30159.1-2013 test method. Place two layers of filter paper on a smooth horizontal surface, and then place the finished fabric flatly on the filter paper with the front side facing up; select the first-grade pressed finished oil that meets GB 1534-2003 as the dirty liquid. Use a dropper to drop about 0.05mL (1 drop) of dirty liquid on each of the three parts of the finished fabric, with a distance of at least 50mm between each drop. When dripping, the dropper mouth is about 6mm away from the surface of the sample. After the sample is left to stand for (30±2)s, observe each drop at an angle of about 45° and rate its grade according to the text description; and record the time from the dirty liquid dripping on the fabric surface to the beginning of wetting.

[0038] The rating standards are shown in Table 2.

[0039] Table 2

[0040]

[0041] Example 1

[0042] In a 500mL beaker, add 42.0g of 3-chloroacryloxypropyl tris(trimethylsiloxy)silane, 6.0g of octadecyl methacrylate, 2.0g of glycidyl methacrylate, 126.3g of deionized water, 10.0g of tripropylene glycol, 5.0g of polyoxyethylene lauryl ether, and 2.0g of octadecyl ammonium chloride, heat to 70°C, and use ultrasound to emulsify and disperse for 10 minutes to obtain a pre-emulsion. The pre-emulsion was transferred to a 500mL reactor, and a solution of 0.2g of dodecyl mercaptan, 0.5g of 2,2-azobis(2-amidinopropane) dihydrochloride (hereinafter referred to as V-50) and 6.0g of deionized water was added. The reaction was carried out at 70°C for 6 hours, and finally the system temperature was lowered to room temperature, and filtered through a 300-mesh filter cloth to obtain an aqueous dispersion of a non-fluorinated polymer.

[0043] Example 2

[0044] In a 500mL beaker, add 40.0g 3-chloroacryloxypropyl tri(trimethylsiloxy)silane, 4.8g stearamide ethyl acrylate, 4.0g methacryloxypropyl heptaisobutyl polysilsesquioxane, 1.2g dimethylaminoethyl methacrylate, 124.3g deionized water, 12.0g tripropylene glycol, 5.0g polyoxyethylene lauryl ether, 2.0g octadecyl ammonium chloride, heat to 70°C, and use ultrasound for 10 minutes of emulsification and dispersion to obtain a pre-emulsion. Transfer the pre-emulsion to a 500mL reactor, add a solution of 0.2g dodecyl mercaptan, 0.5g V-50 and 6.0g deionized water. React at 70°C for 6 hours, finally reduce the system temperature to room temperature, filter through a 300-mesh filter cloth, and obtain an aqueous dispersion of a non-fluorinated polymer.

[0045] Example 3

[0046] In a 500mL beaker, add 42g of methacryloyloxypropyl tris(trimethylsiloxy)silane, 5.8g of 2-(stearylamide)-3-ethyl chloroacrylate, 5.0g of acryloyloxypropyl heptaisobutyl polysilsesquioxane, 1.2g of glycidyl methacrylate, 120.3g of deionized water, 12.0g of dipropylene glycol, 5.0g of polyoxyethylene lauryl ether, and 2.0g of octadecyl ammonium chloride, heat to 70°C, and use ultrasound to emulsify and disperse for 10 minutes to obtain a pre-emulsion. The pre-emulsion is transferred to a 500mL reactor, and a solution of 0.2g of dodecyl mercaptan, 0.5g of V-50 and 6.0g of deionized water is added; react at 70°C for 6 hours, and finally the system temperature is reduced to room temperature, and filtered through a 300-mesh filter cloth to obtain an aqueous dispersion of a non-fluorinated polymer.

[0047] Example 4

[0048] In a 500mL beaker, add 38.0g of methacryloyloxypropyl tris(trimethylsiloxy)silane, 4.8g of (Z)-2-(stearylamide)-2,3-dichloroethyl acrylate (C 18AmClA), 1.2g of 3-chloro-2-hydroxy-propyl methacrylate, 125.7g of deionized water, 10.0g of tripropylene glycol, 4.0g of polyoxyethylene isotridecyl ether, 2.0g of polyoxyethylene dodecyl ether, and 1.6g of octadecyl ammonium chloride, heat to 60°C, and use ultrasound to emulsify and disperse for 10 minutes to obtain a pre-emulsion. The pre-emulsion is transferred to a 500mL autoclave, and a solution of 0.2g of dodecyl mercaptan, 0.5g of V-50 and 6.0g of deionized water is added; the autoclave is then substituted with nitrogen, and 6.0g of vinyl chloride is pressed in. The mixture was reacted at 70° C. for 6 hours, and finally the system temperature was lowered to room temperature and filtered through a 300-mesh filter cloth to obtain an aqueous dispersion of a non-fluorinated polymer.

[0049] Example 5

[0050] In a 500mL beaker, add 42.0g 3-chloroacryloxypropyl triisopropoxysilane, 6.0g octadecyl acrylate, 3.6g 3-chloro-2-hydroxy-propyl methacrylate, 122.1g deionized water, 12.0g dipropylene glycol, 4.0g polyoxyethylene isotridecyl ether, 2.0g polyoxyethylene dodecyl ether, 1.6g octadecyl ammonium chloride, heat to 60°C, and use ultrasound to emulsify and disperse for 10 minutes to obtain a pre-emulsion. The pre-emulsion is transferred to a 500mL reactor, and a solution of 0.2g dodecyl mercaptan, 0.5g V-50 and 6.0g deionized water is added; react at 70°C for 6 hours, and finally the system temperature is reduced to room temperature, and filtered through a 300-mesh filter cloth to obtain an aqueous dispersion of a non-fluorinated polymer.

[0051] Example 6

[0052] 40.0g 3-chloroacryloxypropyl triisopropoxysilane, 6.0g 2-(stearamide)-3-chloroethyl acrylate, 4.0g methacryloxypropyl heptaoctyl polysilsesquioxane, 1.6g 3-chloro-2-hydroxy-propyl methacrylate, 120.1g deionized water, 14.0g tripropylene glycol, 4.0g polyoxyethylene isotridecyl ether, 2.0g polyoxyethylene dodecyl ether, 1.6g octadecyl ammonium chloride were added to a 500mL beaker, heated to 60°C, and emulsified and dispersed for 10 minutes using ultrasound to obtain a pre-emulsion. The pre-emulsion was transferred to a 500mL reactor, and a solution of 0.2g dodecyl mercaptan, 0.5g V-50 and 6.0g deionized water was added; the reaction was carried out at 70°C for 6 hours, and finally the system temperature was lowered to room temperature, and filtered through a 300-mesh filter cloth to obtain an aqueous dispersion of a non-fluorinated polymer.

[0053] Comparative Example 1

[0054] 48.0g 3-methacryloxypropyl triisopropoxysilane, 2.0g glycidyl methacrylate, 124.3g deionized water, 12.0g tripropylene glycol, 5.0g polyoxyethylene lauryl ether, 2.0g octadecyl ammonium chloride were added to a 500mL beaker, heated to 60°C, and emulsified and dispersed for 10 minutes using ultrasound to obtain a pre-emulsion. The pre-emulsion was transferred to a 500mL reactor, and a solution of 0.2g dodecyl mercaptan, 0.5g V-50 and 6.0g deionized water was added; the reaction was carried out at 70°C for 6 hours, and finally the system temperature was lowered to room temperature, and filtered through a 300-mesh filter cloth to obtain an aqueous dispersion of a non-fluorinated polymer.

[0055] Comparative Example 2

[0056] Add 46.0g octadecyl acrylate, 1.2g glycerol methacrylate, 119.1g deionized water, 12.0g dipropylene glycol, 5.0g polyoxyethylene lauryl ether, and 2.0g octadecyl ammonium chloride to a 500mL beaker, heat to 60°C, and use ultrasound to emulsify and disperse for 10 minutes to obtain a pre-emulsion. Transfer the pre-emulsion to a 500mL autoclave, add a solution of 0.2g dodecyl mercaptan, 0.5g V-50, and 6.0g deionized water; then replace the autoclave with nitrogen and press in 8.0g vinyl chloride. React at 70°C for 4 hours, and finally lower the system temperature to room temperature, filter through a 300-mesh filter cloth, and obtain an aqueous dispersion of a non-fluorinated polymer.

[0057] Comparative Example 3

[0058] In a 500mL beaker, 46.0g of methacryloyloxypropyl tris(trimethylsiloxy)silane, 1.6g of 3-chloro-2-hydroxy-propyl methacrylate, 124.1g of deionized water, 14.0g of tripropylene glycol, 4.0g of polyoxyethylene isotridecyl ether, 2.0g of polyoxyethylene dodecyl ether, and 1.6g of octadecyl ammonium chloride were added, heated to 60°C, and emulsified and dispersed for 10 minutes using ultrasound to obtain a pre-emulsion. The pre-emulsion was transferred to a 500mL autoclave, and a solution of 0.2g of dodecyl mercaptan, 0.5g of V-50, and 6.0g of deionized water was added, and the mixture was reacted at 70°C for 6 hours. Finally, the system temperature was lowered to room temperature, and filtered through a 300-mesh filter cloth to obtain an aqueous dispersion of a non-fluorinated polymer.

[0059] The aqueous dispersion of the non-fluoropolymer of Examples 1-6 and Comparative Examples 1-3 was diluted with tap water to a concentration of 30 g / L, and the T / C knitted fabric was dipped and rolled, dried at 100°C, heat treated at 170°C for 60 seconds, and the water repellent effect and stain resistance were measured after rehumidification for 2 hours. The results are shown in Table 3.

[0060] Table 3

[0061]

[0062] The preferred embodiments of the present invention disclosed above are only used to help illustrate the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to the specific implementation methods described. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.

Claims

1. A non-fluorinated polymer, characterized in that The composition comprises the following components by mass percentage: 10% to 40% of a non-fluorine copolymer; 2% to 8% of a surfactant; 2% to 10% of a component; and the balance is deionized water; the non-fluorine copolymer is obtained by polymerizing a silicon-containing acrylate monomer (a), an acrylate monomer (b) having a saturated hydrocarbon group or a cyclic hydrocarbon group with 1 to 30 carbon atoms, and a functional monomer (c) in the presence of a chain transfer agent and a polymerization initiator; the silicon-containing acrylate monomer (a) is a silicon-containing acrylate or a derivative thereof, and its general structural formula is: wherein X1, X2 and X3 are H, CH3, C1 or Br; Y1 is a chemical single bond or one or more of -NH-, -NR2-, -NH-CO-, -NR2-CO-, -NHCONH-, -NHCOO-, -NH-SO2-, -NR2-SO2-; n1 is an integer from 1 to 20; The structural formulas of Z1, Z2 and Z3 are: In the formula, A is a chemical single bond or an oxygen atom, R1, R2 and R3 are saturated hydrocarbon groups or cyclic hydrocarbon groups having 1 to 30 carbon atoms; and m is an integer of 0 to 300.

2. The non-fluorinated polymer according to claim 1, characterized in that The structural formula of the acrylic acid ester monomer (b) having a saturated hydrocarbon group or a cyclic hydrocarbon group having 1 to 30 carbon atoms is: In the formula, X4, X5 and X6 are H, CH3, Cl or Br; R4 represents a saturated hydrocarbon group or a cyclic hydrocarbon group having 1 to 30 carbon atoms; Y2 is a chemical single bond or one or more of -NH-, -NR5-, -NH-CO-, -NR5-CO-, -NHCONH-, -NHCOO-, -NH-SO2-, -NR5-SO2-, R5 is an alkyl group having 1 to 4 carbon atoms; n2 is an integer from 1 to 20.

3. The non-fluorinated polymer according to claim 1, characterized in that The functional monomer (c) is selected from one or more of glycidyl (meth)acrylate, acrylamide, diacetone acrylamide combined with adipic dihydrazide system, ethylene glycol dimethacrylate, trimethylolpropane tri(meth)acrylate, divinylbenzene, dimethylaminoethyl (meth)acrylate, (methoxy)polyethylene glycol (meth)acrylate, (meth)acryloyloxyethyl trimethylammonium chloride, N-acryloyl pyrrolidone, 3-chloro-2-hydroxy-propyl methacrylate, hydroxyethyl (meth)acrylate, hydroxymethyl (meth)acrylate, silicone resin containing reactive groups, vinyl chloride, vinylidene chloride, butadiene, isoprene, and chloroprene.

4. The non-fluorinated polymer according to claim 1, characterized in that The reactive group-containing organic silicone resin is one or more of MQ resin, MT resin, MDT resin or caged polysilsesquioxane (POSS) containing reactive groups, and the reactive groups are one of (meth)acryloyloxy, (meth)acrylamide, vinyl or mercapto.

5. The non-fluorinated polymer according to claim 1, characterized in that The chain transfer agent is alkyl mercaptan; the polymerization initiator is an azo-based, peroxide-based, or redox-based polymerization initiator; and the surfactant contains one or more of a cationic surfactant or a nonionic surfactant.

6. The non-fluorinated polymer according to claim 5, characterized in that The cationic surfactant is one or more of amine, amine salt, quaternary ammonium salt, imidazoline and imidazolinium salt; the nonionic surfactant is one or more of ether, ester, ester ether, alkanolamide, polyol and amine oxide.

7. The non-fluorinated polymer according to claim 1, characterized in that The auxiliary agents include pH adjusting auxiliary agents and organic solvents.

8. The non-fluorinated polymer according to claim 7, characterized in that The pH adjusting agent includes acid, alkali or amino acid, and makes the pH value of the treating agent between 2 and 9.

9. The non-fluorinated polymer according to claim 7, characterized in that The organic solvent is selected from one or a mixture of two of dipropylene glycol, tripropylene glycol, dipropylene glycol ethyl ether, tripropylene glycol ethyl ether, acetone, methyl ethyl ketone, ethyl acetate, n-propyl acetate, butyl acetate, N-methyl-2-pyrrolidone, N,N-dimethylformamide, isopropanol, and n-propanol.

10. A surface treatment agent, characterized in that The non-fluorinated polymer comprises any one of claims 1 to 9.

Citation Information

Patent Citations

  • Water repellent

    CN109923190A

  • High-crosslinking-performance fluorine-free ecological waterproof agent and preparation method thereof

    CN110205818A

  • Silicon-containing fluorine-free waterproofing agent copolymer emulsion for fabrics and polymerization method thereof

    CN110835384A

  • Silicon-containing fluorine-free hydrophobic easily-deterging detergent water-soluble copolymer for fabrics and copolymerization method thereof

    CN110835387A

  • POSS / organosilicon modified polyacrylate fluoride-free waterproof agent and preparation method thereof

    CN112300334A

Cited By

  • Fluorine-free oil-proof agent as well as preparation method and application thereof

    CN119392506A

  • Non-fluorine copolymer as well as preparation method and application thereof

    CN121427030A