Photocuring 3D printing degradable material and preparation method thereof
By modifying the polyimide material with degradability and photocurable properties, combining bio-based compounds and photosensitive diamine monomers, a photocurable 3D printing material with high mechanical and heat resistance is solved, and traditional polyimide is solved. The problem of difficulty in degradation of amine materials and insufficient performance.
Patent Information
- Application Number
- CN202411154496.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-22
- Publication Date
- 2024-11-08
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Traditional polyimide materials are difficult to degrade, and their mechanical properties and photocuring properties are not enough to meet the high requirements of 3D printing materials in the manufacturing and chemical industries.
By modifying the polymeric monomer of polyimide with degradability and photocurability, the degradable dianhydride monomer is synthesized using bio-based compounds, and the grafted photosensitive groups of diamine monomers are synthesized with photosensitivity of grafted photosensitivity groups of diamine monomers Diamine monomers form photocured 3D printing materials with high mechanical properties and degradability properties.
On the basis of ensuring the mechanical properties of polyimide, it improves its photocuring and degradable properties, reduces the system shrinkage rate of parts, and improves the performance of 3D printing materials, especially heat resistance.
Smart Images

Figure FT_1 
Figure FT_2 
Figure FT_3
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of 3D printing materials, and specifically refers to a photocurable 3D printing degradable material and a preparation method thereof. Background Art
[0002] The photocuring 3D printing technology uses ultraviolet light to perform curing scanning on the surface of liquid photocurable resin, so that the photocurable material is cured. The formed photocurable products have the characteristics of high precision, high smoothness and high quality. Photocurable resin is referred to as UV resin, including photosensitive polymer monomers or prepolymers, diluents, photoinitiators and photosensitizers, among which the polymer monomers commonly include ethylene polymers, prepolymers include common polyurethane prepolymers, and diluents include common epoxy compounds. According to the type of photocuring, photocurable resins can be roughly divided into three categories, namely free radical photosensitive resins, cationic photosensitive resins, and photosensitive resins. Ionic photosensitive resin and free radical-cationic hybrid photosensitive resin; free radical photosensitive resin uses acrylate as prepolymer and free radical-type substance as photoinitiator. Under ultraviolet light treatment, the photoinitiator decomposes free radicals, which trigger the double bond transition in acrylate. Polymerization reaction occurs between double bonds to form polymers with large molecular weight. Free radical photosensitive resin has fast curing speed, but there is large system shrinkage, increased internal stress of the product, and easy warping and deformation; cationic photosensitive resin uses epoxy resin as cationic prepolymer. The cationic initiator can decompose effective proton acid to undergo photopolymerization. The mechanical properties of epoxy resin are good. The polymer formed after curing has low internal stress and is not easy to deform. However, the viscosity of epoxy resin is large and the curing rate is slow. Free radical-cationic hybrid photosensitive resin is a mixture of acrylate and epoxy resin. When they interact, cations and free radicals are generated, which can overcome the problems of curing rate and mechanical strength. With the widespread use of 3D printing materials in the manufacturing and chemical industries, 3D printing materials are required to have high precision, high toughness, high strength, high wear resistance and high heat resistance. Polymer materials and petroleum-based materials have the advantages of being biodegradable, recyclable, compostable and incinerable. Bio-based polymer materials mainly include polylactic acid, polyhydroxybutyric acid, polybutylene succinate and polycaprolactone. The degree of biomassization of bio-based polymer materials is high, but affected by the material properties, their thermal stability is poor. Polyimide has a large number of benzene ring molecular structures on the main chain. It is a special engineering plastic with high weather resistance, solvent resistance and wear resistance. However, traditional polyurethane materials have a highly conjugated inductive skeleton molecular structure, which makes its green improvement difficult. Summary of the invention
[0003] In view of the above situation, in order to overcome the defects of the prior art, the present invention provides a photocurable 3D printing degradable material and a preparation method thereof. In order to solve the problem that polyimide materials are difficult to degrade, the present invention uses polyimide as a matrix material, modifies the polymerized monomers of polyimide for degradability and photocurability respectively, synthesizes degradable dianhydride monomers through bio-based compounds, and grafts photosensitive groups onto diamine monomers to synthesize photosensitive diamine monomers. On the basis of ensuring the mechanical properties of polyimide, the photocuring performance and degradability of polyimide can be improved.
[0004] In order to achieve the above-mentioned object, the technical solution adopted by the present invention is as follows: the present invention proposes a photocurable 3D printing degradable material, the degradable material comprising the following components in parts by weight: 45-55 parts of polyimide powder, 23-28 parts of polyvinyl pyrrolidone, 5-10 parts of trimethylolpropane triacrylate, 2-3 parts of IRGACURE 819, and 13-18 parts of N,N-dimethylformamide;
[0005] Preferably, the raw material for preparing the polyimide powder is obtained by reacting a degradable dianhydride monomer and a photosensitive diamine monomer in a mass ratio of 0.55-0.68:1;
[0006] Preferably, the method for preparing the degradable dianhydride monomer specifically comprises the following steps:
[0007] S1. Dilute trimellitic anhydride chloride with dichloromethane, cool in a 4°C ice water bath, and stir for 10-15 minutes to obtain a trimellitic anhydride chloride solution;
[0008] S2, dissolving isosorbide in dichloromethane, adding pyridine and mixing evenly, and then adding dropwise to the trimellitic anhydride chloride solution prepared in step S1 at a rate of 0.75-1 mL / min, raising the temperature of the reaction system to 50-55° C., and performing reflux reaction. After 20-24 hours, the reaction system is cooled to room temperature, filtered, and the filtrate is stirred and washed with deionized water, the organic phase is separated, the dichloromethane is removed, washed, and dried to obtain a degradable dianhydride monomer;
[0009] Preferably, in step S1, the mass concentration of trimellitic anhydride chloride in dichloromethane is 0.2-0.3 g / mL;
[0010] Preferably, in step S2, the mass concentration of isosorbide in dichloromethane is 0.1-0.12 g / mL;
[0011] Preferably, in step S2, the mass ratio between isosorbide and pyridine is 1:1.2-1.5;
[0012] Preferably, in step S2, the mass ratio between isosorbide and trimellitic anhydride chloride is 1:3-3.2;
[0013] Preferably, the method for preparing the photosensitive diamine monomer specifically comprises the following steps:
[0014] S3, 3,5-diaminobenzoic acid is placed in carbon tetrachloride, thionyl chloride is added, mixed evenly, heated to 80-90°C for reflux reaction for 2-3h, thionyl chloride and carbon tetrachloride are removed by vacuum, tetrahydrofuran is added to the reaction system, mixed until the reaction system is uniform, 4-hydroxybutyl acrylate solution is added dropwise, pyridine is added, the reaction is placed in an ice water bath with stirring for 10-12h, and the reaction system is adjusted to neutral with a NaOH solution with a mass fraction of 0.5%, filtered, and the precipitate is dried to obtain a photosensitive diamine monomer;
[0015] Preferably, in step S3, the mass ratio between the 3,5-diaminobenzoic acid and 4-hydroxybutyl acrylate is 1:0.6-0.8;
[0016] Preferably, in step S3, the mass volume ratio g / mL between the 3,5-diaminobenzoic acid and SOCl2 is 2-3 g / mL;
[0017] Preferably, in step S3, the mass concentration of the 3,5-diaminobenzoic acid in carbon tetrachloride is 0.55-0.7 g / mL; the mass concentration of the 4-hydroxybutyl acrylate in tetrahydrofuran is 0.4-0.6 g / mL;
[0018] The present invention provides a method for preparing a photocurable 3D printing degradable material, which specifically comprises the following steps:
[0019] S4, placing a photosensitive diamine monomer in an NMP solvent, stirring until the reactant is completely dissolved, placing the reaction system at 0-4°C, introducing nitrogen, adding a degradable dianhydride monomer solution dropwise to the reaction system, stirring and reacting for 1-1.5 hours, adding maleic anhydride and continuing the reaction for 1-2 hours to obtain a photosensitive degradable polyamic acid solution;
[0020] S5, heating the polyamic acid solution prepared in step S4 to 80-90°C, reacting at a constant temperature for 1.5-2h, raising the temperature to 120-130°C, reacting at a constant temperature for 6-7h, raising the temperature to 200-220°C, reacting at a constant temperature for 5-6h, and after the reaction system is cooled to room temperature, adding deionized water, fully dispersing at 2000-2200rpm, filtering under reduced pressure, collecting the precipitate, washing with deionized water, and vacuum drying to obtain a photosensitive degradable polyimide powder;
[0021] S6. The polyimide powder prepared in step S5, polyvinyl pyrrolidone, trimethylolpropane triacrylate and IRGACURE 819 are mixed in a DMF solvent, placed at 2300-2500 rpm for mixing, and allowed to stand for 20-24 hours to obtain a light-cured 3D printing degradable material.
[0022] Preferably, in step S4, the mass concentration of the photosensitive diamine monomer in the NMP solvent is 55-70 mg / mL; the degradable dianhydride monomer solution is a solution in which the degradable diamine monomer is dissolved in the NMP solvent, and the mass concentration is 60-75 mg / mL;
[0023] Preferably, in step S4, the added mass of maleic anhydride is 9.5%-11.5% of the mass of the photosensitive diamine monomer.
[0024] The beneficial effects achieved by the present invention are as follows:
[0025] The present invention provides a photocurable 3D printing degradable material and a preparation method thereof. The present invention uses polyimide as a matrix material, and modifies the polymerized monomers of the polyimide for degradability and photocurability respectively, synthesizes a degradable dianhydride monomer through a bio-based compound, and grafts a photosensitive group to a diamine monomer to synthesize a photosensitive diamine monomer, thereby improving the photocurability and degradability of the polyimide on the basis of ensuring the mechanical properties of the polyimide; the present invention uses isosorbide as a bio-based compound, and isosorbide is a dehydrated derivative of sorbitol, which has the potential to replace petrochemical raw materials, and reacts trimellitic anhydride chloride with a hydroxyl group of isosorbide to obtain a bio-based monomer substance with a dianhydride structure; uses 3,5-diaminobenzoic acid as an initial raw material, and connects 4-carboxybutylacrylamide with 3,5-diaminobenzoic acid through an esterification reaction, because A double bond group is introduced into the diamine monomer to make it have photocuring performance; a photosensitive diamine monomer and a degradable dianhydride monomer are reacted to form a polyamic acid solution, which is subjected to thermal imidization to form polyimide, and then mixed with an active diluent, a photoinitiator, a cross-linking agent and a solvent to obtain a photocurable 3D printing degradable material. In the 3D printing process, after ultraviolet light irradiation, a solidified layer is formed through a circular path of the laser point, and then the Z axis of the molding platform is lowered to continue to realize the curing of the next layer of resin. After the reaction is completed, the unreacted resin is removed and dried to form a 3D printed part; the polyimide molecular chain has a high content of benzene ring structure, has high mechanical properties, and has high heat resistance. The material prepared by the present invention first synthesizes polyimide and then performs a photocuring reaction, which can reduce the system shrinkage rate of the part and improve the performance of the 3D printing material. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1This is an infrared spectrum image of the photosensitive diamine monomer prepared in Example 1 of the present invention;
[0027] Figure 2 The mechanical properties diagram of the materials prepared in Examples 1-3 and Comparative Examples 1-3;
[0028] Figure 3 It is the TGA curve diagram of the materials prepared in Example 1 and Comparative Examples 1-3.
[0029] The accompanying drawings are used to provide further understanding of the present invention and constitute a part of the specification. They are used to explain the present invention together with the embodiments of the present invention and do not constitute a limitation of the present invention. DETAILED DESCRIPTION
[0030] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments; based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0031] Unless otherwise defined, all professional and scientific terms used herein have the same meanings as those familiar to those skilled in the art. In addition, any methods and materials similar or equivalent to those described herein may be applied to the present invention. The preferred implementation methods and materials described herein are for demonstration purposes only and are not intended to limit the content of this application.
[0032] The experimental methods in the following examples are conventional methods unless otherwise specified; the experimental materials and test strains used in the following examples are purchased from commercial channels unless otherwise specified.
[0033] Example 1
[0034] This embodiment provides a photocurable 3D printing degradable material, comprising the following components in parts by weight: 45 parts of polyimide powder, 28 parts of polyvinyl pyrrolidone, 5 parts of trimethylolpropane triacrylate, 2 parts of IRGACURE 819, and 13 parts of N,N-dimethylformamide;
[0035] The raw materials for preparing the polyimide powder are obtained by reacting a degradable dianhydride monomer and a photosensitive diamine monomer in a mass ratio of 0.68:1;
[0036] The present invention also provides a method for preparing a photocurable 3D printing degradable material, which specifically comprises the following steps:
[0037] S1. Accurately weigh 4.62 g of trimellitic anhydride chloride and place it in a three-necked flask, add 20 mL of dichloromethane to dilute it, place it in a 4°C ice water bath to cool it, and stir it at 50 rpm for 15 minutes to obtain a trimellitic anhydride chloride solution;
[0038] S2. Accurately weigh 1.46 g of isosorbide and place it in a beaker. Add 15 mL of dichloromethane and mix until the isosorbide is completely dissolved. Add 1.8 mL of pyridine and mix. Add the mixture dropwise to the trimellitic anhydride chloride solution prepared in step S1 at a speed of 1 mL / min. Stir evenly at a speed of 100 rpm. Transfer the reaction system to an oil bath. Raise the temperature of the reaction system to 50°C and react for 24 hours. After the reaction system is cooled to room temperature, filter it, collect the filtrate, stir and wash it with deionized water, separate it with a separatory funnel, remove the lower organic phase, remove the water in the organic phase with anhydrous magnesium sulfate, remove dichloromethane with optional evaporation, wash it with deionized water, place it in a vacuum drying oven at 50°C and dry it for 24 hours. Recrystallize it with a mixed solution of acetic acid and acetic anhydride, and purify it to obtain a degradable dianhydride monomer.
[0039] S3. Accurately weigh 20 g of 3,5-diaminobenzoic acid and place it in a flask. Add 30 mL of carbon tetrachloride and 7 mL of SOCl2. After mixing evenly, raise the temperature to 80°C. Maintain the temperature for reflux reaction for 3 hours, evacuate to remove excess reaction solvent, add 50 mL of tetrahydrofuran to the reaction system, fully dissolve the reactants, mix until the reaction system is uniform, stir at 150 rpm in an ice-water bath, accurately weigh 13.5 g of 4-hydroxybutyl acrylate and dissolve it in 27 mL of tetrahydrofuran solvent. Add dropwise to the reaction system at a rate of 3 mL / min, add 10 mL of pyridine, continue stirring and reacting for 10 hours, adjust the reaction system to neutrality with a mass fraction of 0.5% NaOH solution, filter, and place in a vacuum drying oven to dry at 30°C for 10 hours to obtain a photosensitive diamine monomer; molecular weight 338 theoretical constant 31.87 g 90% yield 28.68 g
[0040] The chemical structure of the photosensitive diamine monomer prepared in this example was analyzed using a Fourier transform infrared spectrometer Nicolet Avatar 370. Figure 1 The infrared spectrum image of the photosensitive diamine monomer prepared in Example 1 of the present invention shows a characteristic peak of -NH2 at 3480-3410 cm-1, a characteristic peak of CO in the ester bond at 1240-1190 cm-1, and a characteristic peak of C=C between 1620-1590 cm-1, indicating that an esterification reaction occurred between 3,5-diaminobenzoic acid and 4-hydroxybutyl acrylate;
[0041] S4, placing 1.7 g of photosensitive diamine monomer in a three-necked flask, adding 30 mL of NMP solvent to completely dissolve the photosensitive diamine monomer, placing the flask in a 4°C environment for cooling, accurately weighing 2.5 g of degradable dianhydride monomer and adding it to 40 mL of NMP solvent, after complete dissolution, dripping it into the flask at a rate of 1 mL / min, stirring at a speed of 150 rpm for 1 hour, adding 0.2 g of maleic anhydride, continuing to stir and react for 1 hour, to obtain a photosensitive degradable polyamic acid solution;
[0042] S5, transferring the polyamic acid solution prepared in step S4 to an oil bath, raising the temperature to 90°C under a nitrogen atmosphere, stirring at a constant temperature of 180 rpm for 2 hours, then raising the temperature to 130°C, stirring at a constant temperature of 6 hours, raising the temperature to 220°C, stirring at a constant temperature of 6 hours, and cooling the reaction system to room temperature, adding 100 mL of deionized water, dispersing with a single-phase disperser at a speed of 2000 rpm, collecting the precipitate by filtration under reduced pressure, repeatedly washing with deionized water three times, and drying in a vacuum drying oven at 40°C for 12 hours to obtain a photosensitive degradable polyimide powder;
[0043] S6. The polyimide powder prepared in step S5, polyvinyl pyrrolidone, trimethylolpropane triacrylate and IRGACURE 819 are mixed in a DMF solvent, placed at 2500 rpm for mixing, and allowed to stand for 24 hours to obtain a light-cured 3D printing degradable material.
[0044] Example 2
[0045] This embodiment provides a photocurable 3D printing degradable material, comprising the following components in parts by weight: 50 parts of polyimide powder, 23 parts of polyvinyl pyrrolidone, 8 parts of trimethylolpropane triacrylate, 3 parts of IRGACURE 819, and 15 parts of N,N-dimethylformamide;
[0046] The raw materials for preparing the polyimide powder are obtained by reacting a degradable dianhydride monomer and a photosensitive diamine monomer in a mass ratio of 0.56:1;
[0047] This embodiment provides a method for preparing a photocurable 3D degradable material, which specifically includes the following steps:
[0048] S1. Accurately weigh 7.0 g of trimellitic anhydride chloride and place it in a three-necked flask, add 35 mL of dichloromethane to dilute it, place it in a 4°C ice water bath to cool it, and stir it at 50 rpm for 15 min to obtain a trimellitic anhydride chloride solution;
[0049] S2. Accurately weigh 2.2 g of isosorbide and place it in a beaker. Add 20 mL of dichloromethane and mix until the isosorbide is completely dissolved. Add 3.35 mL of pyridine and mix. Add the mixture dropwise to the trimellitic anhydride chloride solution prepared in step S1 at a speed of 0.8 mL / min. Stir evenly at a speed of 100 rpm. Transfer the reaction system to an oil bath. Raise the temperature of the reaction system to 55 ° C and react for 20 hours. After the reaction system is cooled to room temperature, filter it, collect the filtrate, stir and wash it with deionized water, separate it with a separatory funnel, remove the lower organic phase, remove the water in the organic phase with anhydrous magnesium sulfate, remove dichloromethane with optional evaporation, wash it with deionized water, place it in a 50 ° C vacuum drying oven and dry it for 24 hours. Recrystallize it with a mixed solution of acetic acid and acetic anhydride, and purify it to obtain a degradable dianhydride monomer.
[0050] S3. Accurately weigh 22 g of 3,5-diaminobenzoic acid and place it in a flask, add 40 mL of carbon tetrachloride and 11.3 mL of SOCl2, mix well, raise the temperature to 90°C, maintain the temperature for reflux reaction for 2 hours, evacuate to remove excess reaction solvent, add 50 mL of tetrahydrofuran to the reaction system, fully dissolve the reactants, mix until the reaction system is uniform, stir at 150 rpm in an ice-water bath, accurately weigh 18 g of 4-hydroxybutyl acrylate and dissolve it in 30 mL of tetrahydrofuran solvent, add it dropwise to the reaction system at a speed of 3 mL / min, add 10 mL of pyridine, continue stirring and reacting for 12 hours, adjust the reaction system to neutrality with a 0.5% mass fraction of NaOH solution, filter, and place in a vacuum drying oven to dry at 30°C for 10 hours to obtain a photosensitive diamine monomer;
[0051] S4, placing 1.7 g of photosensitive diamine monomer in a three-necked flask, adding 30 mL of NMP solvent to completely dissolve the photosensitive diamine monomer, placing the flask in a 0°C environment for cooling, accurately weighing 3.0 g of degradable dianhydride monomer and adding it to 40 mL of NMP solvent, after complete dissolution, dripping it into the flask at a rate of 1 mL / min, stirring and reacting at a speed of 150 rpm for 1.5 h, adding 0.2 g of maleic anhydride, continuing to stir and react for 1 h, to obtain a photosensitive degradable polyamic acid solution;
[0052] S5, transferring the polyamic acid solution prepared in step S4 to an oil bath, raising the temperature to 80°C under a nitrogen atmosphere, stirring at a constant temperature of 180 rpm for 1.5 hours, then raising the temperature to 120°C, stirring at a constant temperature for 7 hours, raising the temperature to 200°C, stirring at a constant temperature for 6 hours, and after the reaction system is cooled to room temperature, adding 100 mL of deionized water, dispersing with a single-phase disperser at a speed of 2200 rpm, collecting the precipitate by filtration under reduced pressure, repeatedly washing with deionized water three times, and drying in a vacuum drying oven at 40°C for 12 hours to obtain a photosensitive degradable polyimide powder;
[0053] S6. The polyimide powder prepared in step S5, polyvinyl pyrrolidone, trimethylolpropane triacrylate and IRGACURE 819 are mixed in a DMF solvent, placed at 2300 rpm for mixing, and allowed to stand for 24 hours to obtain a light-cured 3D printing degradable material.
[0054] Example 3
[0055] This embodiment provides a photocurable 3D printing degradable material, comprising the following components in parts by weight: 55 parts of polyimide powder, 25 parts of polyvinyl pyrrolidone, 10 parts of trimethylolpropane triacrylate, 2 parts of IRGACURE 819, and 18 parts of N,N-dimethylformamide;
[0056] The raw materials for preparing the polyimide powder are obtained by reacting a degradable dianhydride monomer and a photosensitive diamine monomer in a mass ratio of 0.67:1;
[0057] This embodiment provides a method for preparing a photocurable 3D degradable material, which specifically includes the following steps:
[0058] S1. Accurately weigh 5.25 g of trimellitic anhydride chloride and place it in a three-necked flask, add 25 mL of dichloromethane to dilute it, place it in a 4°C ice water bath to cool it, and stir it at 50 rpm for 15 min to obtain a trimellitic anhydride chloride solution;
[0059] S2. Accurately weigh 1.75 g of isosorbide and place it in a beaker. Add 15 mL of dichloromethane and mix until the isosorbide is completely dissolved. Add 2.3 mL of pyridine and mix. Add the mixture dropwise to the trimellitic anhydride chloride solution prepared in step S1 at a speed of 1 mL / min. Stir evenly at a speed of 100 rpm. Transfer the reaction system to an oil bath. Raise the temperature of the reaction system to 50°C and react for 24 hours. After the reaction system is cooled to room temperature, filter it, collect the filtrate, stir and wash it with deionized water, separate it with a separatory funnel, remove the lower organic phase, remove the water in the organic phase with anhydrous magnesium sulfate, remove dichloromethane with optional evaporation, wash it with deionized water, place it in a vacuum drying oven at 50°C and dry it for 24 hours. Recrystallize it with a mixed solution of acetic acid and acetic anhydride, and purify it to obtain a degradable dianhydride monomer.
[0060] S3. Accurately weigh 18 g of 3,5-diaminobenzoic acid and place it in a flask, add 30 mL of carbon tetrachloride and 7.4 mL of SOCl2, mix well, raise the temperature to 85°C, maintain the temperature for reflux reaction for 3 hours, evacuate to remove excess reaction solvent, add 50 mL of tetrahydrofuran to the reaction system, fully dissolve the reactants, mix until the reaction system is uniform, stir at 150 rpm in an ice-water bath, accurately weigh 12 g of 4-hydroxybutyl acrylate and dissolve it in 30 mL of tetrahydrofuran solvent, add it dropwise to the reaction system at a speed of 3 mL / min, add 10 mL of pyridine, continue stirring and reacting for 10 hours, adjust the reaction system to neutrality with a 0.5% mass fraction of NaOH solution, filter, and place in a vacuum drying oven to dry at 30°C for 10 hours to obtain a photosensitive diamine monomer;
[0061] S4, placing 2.0 g of photosensitive diamine monomer in a three-necked flask, adding 30 mL of NMP solvent to completely dissolve the photosensitive diamine monomer, placing the flask in a 4°C environment for cooling, accurately weighing 3.0 g of degradable dianhydride monomer and adding it to 40 mL of NMP solvent, after complete dissolution, dripping it into the flask at a rate of 1 mL / min, stirring at a speed of 150 rpm for reaction for 1 hour, adding 0.18 g of maleic anhydride, continuing to stir and react for 2 hours, to obtain a photosensitive degradable polyamic acid solution;
[0062] S5, transferring the polyamic acid solution prepared in step S4 to an oil bath, raising the temperature to 90°C under a nitrogen atmosphere, stirring and reacting at a constant temperature of 180 rpm for 2 hours, then raising the temperature to 120°C, stirring and reacting at a constant temperature of 7 hours, raising the temperature to 220°C, stirring and reacting at a constant temperature of 5 hours, and after the reaction system is cooled to room temperature, adding 100 mL of deionized water and dispersing it with a single-phase disperser at a speed of 2100 rpm, collecting the precipitate by filtration under reduced pressure, repeatedly washing it with deionized water three times, and drying it in a vacuum drying oven at 40°C for 12 hours to obtain a photosensitive degradable polyimide powder;
[0063] S6. The polyimide powder prepared in step S5, polyvinyl pyrrolidone, trimethylolpropane triacrylate and IRGACURE 819 are mixed in a DMF solvent, placed at 2400 rpm for mixing, and allowed to stand for 20 hours to obtain a light-cured 3D printing degradable material.
[0064] Comparative Example 1
[0065] This comparative example provides a photocurable degradable material and a preparation method thereof, which differs from Example 1 only in that the preparation method does not include steps S3 and S4, the degradable dianhydride monomer in step S5 is replaced by 3,5-diaminobenzoic acid of the same molar mass to obtain a polyamic acid solution, the polyamic acid solution is subjected to thermal imidization treatment to form a polyimide solution, 4-hydroxybutyl acrylate is added for modification treatment to obtain a photosensitive modified polyimide, and the remaining components and component contents are the same as those in Example 1.
[0066] Comparative Example 2
[0067] This comparative example provides a photocurable degradable material and a preparation method thereof, which is different from Example 1 in that the degradable dianhydride monomer is replaced by ODPA of the same molar mass, and the remaining components and component contents are the same as those in Example 1.
[0068] Comparative Example 3
[0069] This comparative example provides a polyimide material, which differs from Example 1 in that the degradable dianhydride monomer is replaced by ODPA of the same molar mass, and the photosensitive diamine monomer is replaced by 6FAP of the same molar mass. After a polyamic acid solution is prepared according to the reaction in step S5, polyimide is formed by thermal imidization.
[0070] Experimental Example 1
[0071] In this experimental example, the mechanical properties of the photocurable degradable materials prepared in Examples 1-3 and Comparative Examples 1-3 were measured. The photocurable degradable materials prepared in Examples 1-3 and Comparative Examples 1-2 were coated with a coating thickness of 300 μm. After UV curing for 15 minutes, the coating was placed at 220° C. for drying to obtain a photocurable degradable material sample. The polyimide prepared in Comparative Example 3 was coated and then placed at 220° C. for heat treatment to obtain a polyimide sample. The depth of the test material being pressed was measured by a nanoindenter, and the load was set to 3 mN. The hardness and Young's modulus of the material were calculated.
[0072] Figure 2 The mechanical properties diagram of the materials prepared in Examples 1-3 and Comparative Examples 1-3 are as shown in the figure. The hardness and modulus of the materials prepared in Examples 1-3 are significantly higher than those of the materials prepared in Comparative Example 1. Comparative Example 2 sacrifices the degradable performance, replaces the degradable dianhydride monomer with ODPA, and introduces a more rigid benzene ring structure into the molecular chain of the material, but the mechanical properties of the materials prepared in Comparative Example 2 are slightly different from those of the materials prepared in Examples 1-3. Comparative Example 3 is a polyimide material, and its hardness and modulus are maintained at a high level, but the difference with the materials prepared in the examples is small, indicating that the photocurable 3D degradable material prepared by the present invention retains the higher mechanical properties of the polyimide material, while modifying its degradability and photocurability.
[0073] Experimental Example 2
[0074] In this experimental example, the thermal stability of the materials prepared in Example 1 and Comparative Examples 1-3 was tested. A synchronous thermal analyzer was used to place the samples in an Al2O3 crucible. The temperature was raised at a rate of 10°C / min from room temperature to 850°C in a nitrogen atmosphere, and the thermal weight loss rate was measured.
[0075] Figure 3The TGA curves of the materials prepared in Example 1 and Comparative Examples 1-3 are as shown in the figure. Image 1 is the TGA image of the material prepared in Example 1, Image 2 is the TGA image of the material prepared in Comparative Example 1, Image 3 is the TGA image of the material prepared in Comparative Example 2, and Image 4 is the TGA image of the material prepared in Example 3. When the temperature rises to 170°C-180°C, the materials prepared in Example 1 and Comparative Examples 1-2 experience different degrees of weight loss. The CO bond fails due to the increase in temperature, and the formed CO2 volatilizes. At the same time, the solvent in the molecular molecules also volatilizes, and the materials prepared in Example 1 and Comparative Examples 1-3 produce obvious weight loss at 400-600°C, which is caused by the breakage of the aromatic ring. Similarly, due to the addition of polyvinyl pyrrolidone and trimethylolpropane triacrylate in Example 1 and Comparative Examples 1-2, the heat resistance decreases, but Example 1 can maintain a weight loss rate equivalent to that of polyimide, indicating that the photocurable 3D degradable material prepared by the present invention has high heat resistance.
[0076] While the embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that many changes, modifications, substitutions and variations can be made to the embodiments without departing from the principles and spirit of the invention.
[0077] The present invention and its implementation methods are described above, but such description is not restrictive. The drawings show only one implementation method of the present invention, and the actual application is not limited thereto. In short, if ordinary technicians in the field are inspired by it, without departing from the purpose of the invention, the methods and embodiments similar to the technical solution without creative design should all fall within the protection scope of the present invention.
Claims
1. A photocurable 3D printing biodegradable material, characterized in that: The degradable material comprises the following components in parts by weight: 45-55 parts of polyimide powder, 23-28 parts of polyvinyl pyrrolidone, 5-10 parts of trimethylolpropane triacrylate, 2-3 parts of IRGACURE 819, and 13-18 parts of N,N-dimethylformamide; the raw materials for preparing the polyimide powder are obtained by reacting a degradable dianhydride monomer and a photosensitive diamine monomer in a mass ratio of 0.55-0.68:
1.
2. A method for preparing a photocurable 3D printing degradable material according to claim 1, characterized in that: The preparation method of the degradable dianhydride monomer specifically comprises the following steps: S1. Dilute trimellitic anhydride chloride with dichloromethane, cool in a 4°C ice water bath, and stir for 10-15 minutes to obtain a trimellitic anhydride chloride solution; S2. Dissolve isosorbide in dichloromethane, add pyridine and mix well, then add dropwise to the trimellitic anhydride chloride solution prepared in step S1 at a rate of 0.75-1 mL / min, and raise the temperature of the reaction system to 50-55° C. for reflux reaction. After 20-24 hours, cool the reaction system to room temperature, filter, wash the filtrate with deionized water, separate the organic phase, remove dichloromethane, wash, and dry to obtain a degradable dianhydride monomer.
3. The method for preparing a photocurable 3D printing degradable material according to claim 2, characterized in that: The preparation method of the photosensitive diamine monomer specifically comprises the following steps: S3. Place 3,5-diaminobenzoic acid in carbon tetrachloride, add thionyl chloride, mix well, heat to 80-90°C for reflux reaction for 2-3h, remove thionyl chloride and carbon tetrachloride by vacuum, add tetrahydrofuran into the reaction system, mix until the reaction system is uniform, drop 4-hydroxybutyl acrylate solution, add pyridine, place in an ice water bath and stir for 10-12h, adjust the reaction system to neutral with 0.5% by mass NaOH solution, filter, take the precipitate and dry it to obtain a photosensitive diamine monomer.
4. The method for preparing a photocurable 3D printing degradable material according to claim 3, characterized in that: The specific steps include: S4, placing a photosensitive diamine monomer in an NMP solvent, stirring until the reactant is completely dissolved, placing the reaction system at 0-4°C, introducing nitrogen, adding a degradable dianhydride monomer solution dropwise to the reaction system, stirring and reacting for 1-1.5 hours, adding maleic anhydride and continuing the reaction for 1-2 hours to obtain a photosensitive degradable polyamic acid solution; S5, heating the polyamic acid solution prepared in step S4 to 80-90°C, reacting at a constant temperature for 1.5-2h, raising the temperature to 120-130°C, reacting at a constant temperature for 6-7h, raising the temperature to 200-220°C, reacting at a constant temperature for 5-6h, and after the reaction system is cooled to room temperature, adding deionized water, fully dispersing at 2000-2200rpm, filtering under reduced pressure, collecting the precipitate, washing with deionized water, and vacuum drying to obtain a photosensitive degradable polyimide powder; S6. Mix the polyvinyl pyrrolidone, trimethylolpropane triacrylate and IRGACURE 819 prepared in step S5 in a DMF solvent, place the mixture at 2300-2500 rpm, and let stand for 20-24 hours to obtain a light-cured 3D printing degradable material.
5. The method for preparing a photocurable 3D printing degradable material according to claim 4, characterized in that: In step S1, the mass concentration of trimellitic anhydride chloride in dichloromethane is 0.2-0.3 g / mL.
6. The method for preparing a photocurable 3D printing degradable material according to claim 5, characterized in that: In step S2, the mass ratio of isosorbide to trimellitic anhydride chloride is 1:3-3.2; the mass ratio of isosorbide to pyridine is 1:1.2-1.5; and the mass concentration of isosorbide in dichloromethane is 0.1-0.12 g / mL.
7. The method for preparing a photocurable 3D printing degradable material according to claim 6, characterized in that: In step S3, the mass ratio of the 3,5-dinitrobenzoic acid to 4-hydroxybutyl acrylate is 1:0.6-0.8; in step S3, the mass volume ratio of the 3,5-dinitrobenzoic acid to SOCl2 is 2-3 g / mL.
8. The method for preparing a photocurable 3D printing degradable material according to claim 7, characterized in that: In step S3, the mass concentration of the 3,5-dinitrobenzoic acid in carbon tetrachloride is 0.55-0.7 g / mL; the mass concentration of the 4-hydroxybutyl acrylate in tetrahydrofuran is 0.4-0.6 g / mL.
9. The method for preparing a photocurable 3D printing degradable material according to claim 8, characterized in that: In step S4, the mass concentration of the photosensitive diamine monomer in the NMP solvent is 55-70 mg / mL; the degradable dianhydride monomer solution is a solution of the degradable diamine monomer dissolved in the NMP solvent, and the mass concentration is 60-75 mg / mL; the added mass of the maleic anhydride is 9.5%-11.5% of the mass of the photosensitive diamine monomer.