Mud-resistant polycarboxylate superplasticizer and preparation method thereof

By preparing a mud-resistant polycarboxylate superplasticizer containing phosphate and quaternary ammonium salt groups, the problem of decreased dispersibility of polycarboxylate superplasticizer in sand and gravel with high mud content was solved, thus improving the workability and fluidity of concrete.

CN118909204AActive Publication Date: 2024-11-08POLY CHANGDA ENGINEERING CO LTD +2
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411199134.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-11-08
Estimated Expiration
2044-08-29

AI Technical Summary

Technical Problem

Existing polycarboxylate superplasticizers have poor adaptability to sand and gravel with high mud content, resulting in decreased workability of concrete. There is a lack of superplasticizers suitable for sand and gravel with high mud content.

Method used

A mud-resistant polycarboxylate superplasticizer was prepared by copolymerization of unsaturated polyether macromonomers, acrylic acid, unsaturated phosphite amphoteric monomers, initiators, and chain transfer agents. The molecular structure contains phosphite and quaternary ammonium salt groups, which enhances its adsorption capacity and dispersibility in soil.

Benefits of technology

It improves the dispersibility and flowability of polycarboxylate superplasticizer, enhances its resistance to soil, and improves the workability and slump retention of concrete.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_11
    Figure SMS_11
  • Figure SMS_12
    Figure SMS_12
  • Figure SMS_13
    Figure SMS_13
Patent Text Reader

Abstract

The invention discloses a mud-resistant polycarboxylate superplasticizer and a preparation method thereof, and belongs to the field of concrete. The mud-resistant polycarboxylate superplasticizer is prepared from the following raw materials in percentage by mole: 15%-25% of unsaturated polyether macromonomer, 60%-80% of acrylic acid, 1%-10% of unsaturated phosphite amphoteric monomer, 0.5%-5% of initiator, 0.01%-0.5% of chain transfer agent and the balance of water. The mud-resistant polycarboxylate superplasticizer provided by the invention has good dispersity and dispersion retentivity, so that the mud-resistant polycarboxylate superplasticizer has excellent mud resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of concrete, and in particular to an anti-mud type polycarboxylate water reducer and a preparation method thereof. Background Art

[0002] In the actual production and application of concrete, it is found that with the sharp increase in domestic infrastructure projects, a large amount of high-quality concrete raw materials are consumed. In addition, with the increasing pressure on environmental protection, the amount of raw materials mined is gradually decreasing and the price is rising year by year. Therefore, more and more concrete construction projects are forced to use poor quality sand and gravel with a high mud content.

[0003] Polycarboxylate superplasticizer (PCE) is very sensitive to the mud content of sand and gravel in concrete, mainly because the mud content will affect the workability of fresh concrete. When the sand and gravel contain no mud or low mud content, the polycarboxylate superplasticizer has very superior performance, but once the mud content in the sand and gravel increases, the performance of the polycarboxylate superplasticizer will drop significantly. The mud components in sand and gravel do not all have an inhibitory effect on polycarboxylate superplasticizer. A large number of studies have found that the influence of clay minerals in the mud on polycarboxylate superplasticizer is the main reason. Clay is mostly layered silicate minerals. The characteristic of this type of mineral is that there are interlayer domains between the lamellar layers that constitute the unit structure. After absorbing water, the volume expands and the size becomes larger, and water molecules and polycarboxylic acid molecules are absorbed into them, resulting in a further reduction in the amount of water in the system, and the polycarboxylate superplasticizer molecules used to disperse cement particles are occupied by clay, which affects the workability of the entire concrete system.

[0004] As the mud content in sand and gravel increases, a large amount of polycarboxylate water-reducing agent is adsorbed during use, which reduces the dispersibility and dispersion retention of the polycarboxylate water-reducing agent, resulting in a decrease in the working performance of the concrete. Therefore, there is a lack of a polycarboxylate water-reducing agent suitable for sand and gravel with high mud content. Summary of the invention

[0005] In view of the above-mentioned deficiencies in the prior art, the present invention proposes an anti-mud polycarboxylate water reducer and a preparation method thereof to solve the problem of the current lack of a polycarboxylate water reducer suitable for sand and gravel with high mud content.

[0006] To achieve the above object, the present invention provides an anti-mud type polycarboxylate water reducer. The raw materials for preparing the anti-mud type polycarboxylate water reducer include, by mole percentage, 15% to 25% of an unsaturated polyether macromonomer, 60% to 80% of acrylic acid, 1% to 10% of an unsaturated phosphite amphoteric monomer, 0.5% to 5% of an initiator, 0.01% to 0.5% of a chain transfer agent, and the balance is water.

[0007] Optionally, the structure of the unsaturated phosphite amphoteric monomer is as shown in formula (I): (I).

[0008] Optionally, the molecular weight of the unsaturated polyether macromonomer is 1000-3000.

[0009] Optionally, the unsaturated polyether macromonomer includes at least one of allyl polyoxyethylene ether, isobutylene alcohol polyoxyethylene ether, and isopentyl polyoxyethylene ether.

[0010] Optionally, the initiator includes at least one of hydrogen peroxide, ammonium persulfate or potassium persulfate.

[0011] Optionally, the chain transfer agent is selected from at least one of mercaptopropionic acid, thioglycolic acid, sodium methyl methacrylate sulfonate or sodium propylene sulfonate.

[0012] Optionally, the chemical structural formula of the anti-mud polycarboxylate water-reducing agent is as shown in formula (II): (II), where R 1 -H or -CH 3 ; R 2 -CH 2 -or-CH 2 CH 2 -; y, z, m, and n are all non-zero integers.

[0013] In order to achieve the above object, the present invention also proposes a method for preparing the above-mentioned anti-mud type polycarboxylate water-reducing agent, comprising the following steps: S1: copolymerizing the unsaturated polyether macromonomer, acrylic acid, unsaturated phosphite amphoteric monomer, initiator and chain transfer agent with water to obtain a copolymer solution; S2: cooling the copolymer solution, and then adjusting the pH value with an alkaline substance to obtain a clear solution, which is the anti-mud type polycarboxylate water-reducing agent.

[0014] Optionally, the copolymerization reaction is carried out at 50° C. to 70° C. for 3 hours to 5 hours.

[0015] Optionally, the cooling is to below 40°C.

[0016] The beneficial effects of the present invention are as follows: the anti-mud polycarboxylate water-reducing agent provided by the present invention contains both phosphite and quaternary ammonium salt groups on the molecular side chains, has stronger adsorption capacity than the existing polycarboxylate water-reducing agent, can effectively resist sulfate in cement, and at the same time, the positively charged groups carried by the quaternary ammonium salt groups produce adsorption on soil, reduce the influence of soil on cement particles, greatly improve the dispersibility and fluidity of the polycarboxylate water-reducing agent, and the phosphite structure can also change the crystal morphology formed in the early stage of calcium sulfonate to improve the collapse retention performance; at the same time, the synergistic effect of the carboxyl, phosphite, hydroxyl and quaternary ammonium salt groups contained in the water-reducing agent molecular chain is conducive to the wetting and adsorption of the cement and soil particle surfaces and the relative lubrication between aggregate particles, so that the anti-mud polycarboxylate water-reducing agent has good dispersibility and dispersion retention, and shows good mud resistance. DETAILED DESCRIPTION

[0017] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below. It should be understood that the following embodiments are only used to explain the present invention and are not used to limit the present invention.

[0018] Unless defined otherwise, all technical and scientific terms used herein have the common meaning in the art to which the claimed subject matter belongs.

[0019] In the actual production and application of concrete, it is found that with the sharp increase in domestic infrastructure projects, a large amount of high-quality concrete raw materials are consumed. In addition, with the increasing pressure on environmental protection, the amount of raw materials mined is gradually decreasing and the price is rising year by year. Therefore, more and more concrete construction projects are forced to use poor quality sand and gravel with a high mud content.

[0020] Polycarboxylate superplasticizer (PCE) is very sensitive to the mud content of sand and gravel in concrete, mainly because the mud content will affect the workability of fresh concrete. When the sand and gravel contain no mud or low mud content, the polycarboxylate superplasticizer has very superior performance, but once the mud content in the sand and gravel increases, the performance of the polycarboxylate superplasticizer will drop significantly. The mud components in sand and gravel do not all have an inhibitory effect on polycarboxylate superplasticizer. A large number of studies have found that the influence of clay minerals in the mud on polycarboxylate superplasticizer is the main reason. Clay is mostly layered silicate minerals. The characteristic of this type of mineral is that there are interlayer domains between the lamellar layers that constitute the unit structure. After absorbing water, the volume expands and the size becomes larger, and water molecules and polycarboxylic acid molecules are absorbed into them, resulting in a further reduction in the amount of water in the system, and the polycarboxylate superplasticizer molecules used to disperse cement particles are occupied by clay, which affects the workability of the entire concrete system.

[0021] As the mud content in sand and gravel increases, a large amount of polycarboxylate water-reducing agent is adsorbed during use, which reduces the dispersibility and dispersion retention of the polycarboxylate water-reducing agent, resulting in a decrease in the working performance of the concrete. Therefore, there is a lack of a polycarboxylate water-reducing agent suitable for sand and gravel with high mud content.

[0022] In order to solve the above problems, the present invention provides an anti-mud type polycarboxylate water reducer. The raw materials for preparing the anti-mud type polycarboxylate water reducer include, by mole percentage, 15% to 25% of an unsaturated polyether macromonomer, 60% to 80% of acrylic acid, 1% to 10% of an unsaturated phosphite amphoteric monomer, 0.5% to 5% of an initiator, 0.01% to 0.5% of a chain transfer agent, and the balance is water.

[0023] The anti-mud polycarboxylate water-reducing agent of the present invention is a copolymer prepared by free radical copolymerization reaction of unsaturated polyether macromonomer, unsaturated phosphite amphoteric monomer and acrylic acid as raw materials in the presence of an initiator and a chain transfer agent.

[0024] As the skeleton of the copolymer, the unsaturated polyether macromonomer provides stability and certain flexibility of the molecular structure, which helps to improve the adsorption capacity and dispersibility of the water reducer. The steric hindrance effect of the macromonomer helps to disperse the water reducer between cement particles, avoid cement flocculation, and thus improve the fluidity of the concrete.

[0025] Acrylic acid is the main monomer. The carboxyl functional group of acrylic acid forms an adsorption layer on the surface of cement particles, enhancing the water-reducing effect. A high content of acrylic acid helps to increase the acidity of the water reducer, promote cement hydration reaction, and improve the early strength of concrete.

[0026] Unsaturated phosphite amphoteric monomers introduce phosphorus elements, provide zwitterionic properties, and enhance the interaction between the water reducer and cement and soil. The amphoteric monomers may improve the mud resistance and dispersion stability of the water reducer by forming more chemical adsorption and physical entanglement.

[0027] The initiator initiates the free radical copolymerization reaction, controls the initiation and rate of the polymerization reaction, and ensures the smooth progress of the reaction.

[0028] Chain transfer agents adjust the molecular weight and molecular weight distribution of polymers to avoid the decrease in solubility and dispersibility caused by too high molecular weight. Chain transfer agents can control polymerization reactions, reduce overpolymerization of polymers, and ensure the stability and long-term storage performance of water reducers.

[0029] Through reasonable raw material ratio and polymerization process, the mud-resistant polycarboxylate water-reducing agent prepared has excellent mud resistance while maintaining high water-reducing performance. The molecular structure design of the polymer helps to improve its adsorption capacity on the surface of cement particles and reduce the influence of clay and other soil on the water-reducing effect. The high content of acrylic acid gives the water-reducing agent a strong acidity, promotes cement hydration, and improves the early strength and workability of concrete. The introduction of unsaturated phosphite amphoteric monomers enhances the interaction between the water-reducing agent and cement and soil, and improves the mud resistance and stability of the water-reducing agent. The precise control of the initiator and chain transfer agent ensures the molecular weight and molecular weight distribution of the polymer, thereby ensuring the solubility, dispersibility and storage stability of the water-reducing agent.

[0030] Furthermore, the structure of the unsaturated phosphite amphoteric monomer is shown in formula (I): (I). The introduction of phosphate groups effectively weakens the adsorption of mud on carboxyl groups, thereby improving the tolerance of the water reducer in materials with a high mud content, solving the problem of reduced performance of traditional polycarboxylate water reducers in the presence of mud. At the same time, the phosphate group has a stronger ability to complex with calcium ions in cement, which improves the dispersibility of the water reducer and makes the concrete have better fluidity and workability. In addition, the phosphite structure of this scheme is also conducive to changing the crystal morphology formed in the early stage of calcium sulfonate and thus improving the collapse retention performance.

[0031] Further, the molecular weight of the unsaturated polyether macromonomer is 1000-3000. The unsaturated polyether macromonomer within this molecular weight range has a high polymerization reaction activity. More preferably, the molecular weight of the unsaturated polyether macromonomer is 2200-2500. More preferably, the molecular weight of the unsaturated polyether macromonomer is 2400.

[0032] Further, the unsaturated polyether macromonomer includes at least one of allyl polyoxyethylene ether, isobutylene alcohol polyoxyethylene ether, and isopentyl polyoxyethylene ether. These unsaturated polyether macromonomers can affect the molecular weight, molecular weight distribution, and regularity of the molecular structure of the final polymer during the polymerization process due to their different carbon chain lengths and structures. Different macromonomers can provide different steric hindrances and hydrophilic / hydrophobic balances, which are crucial for the adsorption and dispersion effects of the water reducer on cement particles. By reasonably matching these macromonomers, polycarboxylate water reducers with excellent comprehensive properties can be obtained, such as high water reduction rate, good cement adaptability, low shrinkage, high durability, etc., and these macromonomers have high double bond retention rates and good activity, which are suitable for preparing the polycarboxylate water reducer of this scheme.

[0033] Furthermore, the initiator includes at least one of hydrogen peroxide, ammonium persulfate or potassium persulfate. These initiators can effectively decompose and generate free radicals to initiate the polymerization reaction of the polycarboxylate water-reducing agent polymer, have a wide temperature application range, good stability, and high safety. At the same time, the decomposition rate and reaction conditions of these initiators are relatively easy to control, which helps to obtain the expected degree of polymerization and molecular weight distribution.

[0034] Furthermore, the chain transfer agent is selected from at least one of mercaptopropionic acid, thioglycolic acid, sodium methyl methacrylate sulfonate or sodium propylene sulfonate.

[0035] Furthermore, the chemical structural formula of the anti-mud polycarboxylate water-reducing agent is as shown in formula (II): (II), where R 1 -H or -CH 3 ; R 2 -CH 2 -or-CH 2 CH 2 -; y, z, m, n are all non-zero integers. The molecular side chains of this solution contain both phosphite and quaternary ammonium salt groups, which have stronger adsorption capacity than existing polycarboxylate water reducers and can effectively resist sulfate in cement. At the same time, the positively charged groups carried by the quaternary ammonium salt groups produce adsorption on soil, reducing the influence of soil on cement particles, greatly improving the dispersibility and fluidity of the polycarboxylate water reducer, and the phosphite structure can also change the crystal morphology formed in the early stage of calcium sulfonate and thus improve the collapse retention performance; at the same time, the synergistic effect of the carboxyl, phosphite, hydroxyl and quaternary ammonium salt groups contained in the molecular chain of the water reducer is beneficial to its wetting and adsorption on the surface of cement and soil particles and the relative lubrication between aggregate particles, so that the anti-mud polycarboxylate water reducer has good dispersibility and dispersion retention, showing good anti-mud performance.

[0036] In some embodiments, R 1 -CH 3 And R 2 -CH 2 CH 2 -.

[0037] In order to solve the above problems, the present invention also proposes a method for preparing the above anti-mud type polycarboxylate water-reducing agent, comprising the following steps: S1: copolymerizing the unsaturated polyether macromonomer, acrylic acid, unsaturated phosphite amphoteric monomer, initiator and chain transfer agent with water to obtain a copolymer solution; S2: Cooling the copolymer solution, and then adjusting the pH value with an alkaline substance to obtain a clear solution, which is the anti-mud polycarboxylate water-reducing agent. In some embodiments, the pH value is adjusted to be in the range of 6.0-7.0.

[0038] Furthermore, the copolymerization reaction is carried out at 50°C to 70°C for 3 hours to 5 hours. In a further preferred embodiment, the copolymerization reaction temperature in S1 is 57 to 60°C.

[0039] Furthermore, the cooling is to below 40°C.

[0040] The method for preparing the anti-mud polycarboxylate water reducer of the present invention achieves high performance and improved stability of the water reducer by precisely controlling the copolymerization reaction conditions and pH value adjustment. The method carries out a copolymerization reaction at 50°C to 70°C for 3 to 5 hours to ensure the uniformity and activity of the polymer, and then obtains a clear and stable water reducer solution by cooling to below 40°C and adjusting the pH value to 6.0-7.0. The water reducer has excellent anti-mud performance, enhances the interaction with cement and soil, and maintains the characteristics of environmental friendliness and easy operation.

[0041] The present invention is further described in detail below in conjunction with specific embodiments.

[0042] Embodiment 1: Add 250g of water and 300g of polyether macromonomer APEG to a 1000mL four-necked round-bottom flask equipped with a thermometer, an electric stirrer, a constant temperature electric heating jacket, and a peristaltic pump. The molecular weight of the APEG used is 2400. Stir and heat to 58°C. After dissolving evenly, directly add a mixed solution of 3.9g of hydrogen peroxide and 16g of water and stir for 10 minutes to fully dissolve it. Add a mixed aqueous solution consisting of 45g of acrylic acid, 15g of unsaturated phosphite amphoteric monomer, and 76g of water and a mixed solution consisting of 0.60g of ascorbic acid, 1.6g of mercaptopropionic acid, and 90g of water dropwise within 3 hours, and keep the temperature between 57-60°C; after the addition is completed, continue to react for 2 hours, then cool to 30-35°C, add 30% sodium hydroxide solution and dilution water, and obtain an anti-mud polycarboxylic acid water reducer with a pH of 6-7 and a concentration of about 40%, and its structural formula is: .

[0043] Embodiment 2: Add 250g of water and 300g of polyether macromonomer HPEG to a 1000mL four-necked round-bottom flask equipped with a thermometer, an electric stirrer, a constant temperature electric heating jacket, and a peristaltic pump. The molecular weight of the HPEG used is 2400. Stir and heat to 58°C. After dissolving evenly, directly add a mixed solution of 3.9g of hydrogen peroxide and 16g of water and stir for 10 minutes to fully dissolve it. Add a mixed aqueous solution consisting of 45g of acrylic acid, 15g of unsaturated phosphite amphoteric monomer, and 76g of water and a mixed solution consisting of 0.60g of ascorbic acid, 1.6g of mercaptopropionic acid, and 90g of water dropwise within 3 hours, and keep the temperature between 57-60°C; after the addition is completed, continue to react for 2 hours, then cool to 35-40°C, add 30% sodium hydroxide solution and dilution water, and obtain an anti-mud polycarboxylic acid water reducer with a pH of 6-7 and a concentration of about 40%, and its structural formula is: .

[0044] Embodiment 3: Add 250g of water and 300g of polyether macromonomer TPEG to a 1000mL four-necked round-bottom flask equipped with a thermometer, an electric stirrer, a constant temperature electric heating jacket, and a peristaltic pump. The molecular weight of the TPEG used is 2400. Stir and heat to 58°C. After dissolving evenly, directly add a mixed solution of 3.9g of hydrogen peroxide and 16g of water and stir for 10 minutes to fully dissolve it. Add a mixed aqueous solution consisting of 45g of acrylic acid, 15g of unsaturated phosphite amphoteric monomer, and 76g of water and a mixed solution consisting of 0.60g of ascorbic acid, 1.6g of mercaptopropionic acid, and 90g of water dropwise within 3 hours, and keep the temperature between 57-60°C; after the addition is completed, continue to react for 2 hours, then cool to 35-40°C, add 30% sodium hydroxide solution and dilution water, and obtain an anti-mud polycarboxylic acid water reducer with a pH of 6-7 and a concentration of about 40%, and its structural formula is: .

[0045] Embodiment 4: Add 250g of water and 300g of polyether macromonomer TPEG to a 1000mL four-necked round-bottom flask equipped with a thermometer, an electric stirrer, a constant temperature electric heating jacket, and a peristaltic pump. The molecular weight of the TPEG used is 2400. Stir and heat to 58°C. After uniform dissolution, directly add a mixed solution of 4.6g of hydrogen peroxide and 16g of water and stir for 10 minutes to fully dissolve it. Add a mixed aqueous solution consisting of 40g of acrylic acid, 20g of unsaturated phosphite amphoteric monomer, and 80g of water and a mixed solution consisting of 0.53g of ascorbic acid, 1.44g of mercaptopropionic acid, and 80g of water dropwise within 3 hours, and keep the temperature between 57-60°C; after the addition is completed, continue to react for 2 hours, then cool to 35-40°C, add 30% sodium hydroxide solution and dilution water, and obtain an anti-mud polycarboxylic acid water reducer with a pH of 6-7 and a concentration of about 40%, and its structural formula is:

[0046] Comparative Example 1 In a 1000mL four-necked round-bottom flask equipped with a thermometer, an electric stirrer, an electric heating jacket, and a peristaltic pump, add 250g of water and 300g of a polyether macromonomer HPEG, the molecular weight of which is 2400. After stirring and dissolving evenly, directly add 3.9g of a hydrogen peroxide solution and stir for 10 minutes to fully dissolve it. Within 3 hours and 3.5 hours, respectively, add a mixed aqueous solution consisting of 45g of acrylic acid and 60g of water and a mixed solution consisting of 1.6g of ascorbic acid, 2.0g of mercaptopropionic acid, and 60g of water, and add dropwise at room temperature; after the addition is completed, continue to react for 1 hour, add 30% sodium hydroxide solution and dilution water, and obtain a conventional polycarboxylic acid water reducer with a pH of 6-7 and a concentration of about 40%, and its structural formula is: .

[0047] Comparative Example 2 Add 250g of water and 300g of polyether macromonomer TPEG to a 1000mL four-necked round-bottom flask equipped with a thermometer, an electric stirrer, an electric heating jacket, and a peristaltic pump. The molecular weight of the TPEG used is 2400. After stirring and dissolving evenly, directly add a mixed solution of 3.9g of hydrogen peroxide and 16g of water and stir for 10 minutes to fully dissolve it. Add a mixed aqueous solution consisting of 42g of acrylic acid and 60g of water and a mixed solution consisting of 1.6g of ascorbic acid, 2.0g of mercaptopropionic acid, and 60g of water dropwise within 2 hours and 2.5 hours, respectively, at room temperature; continue to react for 1.5 hours after the addition is completed, add 30% sodium hydroxide solution and dilution water, and obtain a conventional polycarboxylic acid water reducer with a pH of 6-7 and a concentration of about 40%, and its structural formula is: .

[0048] Further, the above-mentioned Examples 1 to 4 and Comparative Example 1 were tested for the flow of the pure paste according to GB / T 8077-2012 "Test Method for Homogeneity of Concrete Admixtures", with cement as the reference cement, and the test results are shown in Table 1; the above-mentioned Examples 1 to 4 and Comparative Example 1 were tested with reference to GB / T 50080-2002 "Standard for Test Method for Performance of Ordinary Concrete Mixtures", and the slump and expansion at the initial and 60 minutes were tested. The mix ratio of C30 machine-made sand concrete is shown in Table 2, Conch Cement, machine-made sand, Grade II fly ash, fineness modulus 3.2, stone powder content 7.2%, MB value 2.1, and mud is the main component of the stone powder. The concrete test results are shown in Table 3.

[0049] Table 1 Test results of cement paste fluidity

[0050] Table 2 Mix ratio of C30 machine-made sand concrete

[0051] Table 3 Concrete test results

[0052] It can be seen from the data in Table 1 that, at the same water reducer dosage and bentonite amount, the initial fluidity of Examples 1 to 4 (the anti-mud polycarboxylate water reducer of the present invention) is about 260 mm, while the initial fluidity of Comparative Examples 1 to 2 (conventional polycarboxylate water reducer) is about 220 mm. The 90-min cement paste fluidity of Examples 1 to 4 is about 190 mm, while Comparative Examples 1 to 2 have no fluidity at 90 minutes. This shows that the anti-mud polycarboxylate water reducer of the present invention has excellent water reduction, slump retention and anti-mud performance, and is significantly better than conventional polycarboxylate water reducers.

[0053] As can be seen from Table 3, Examples 1 to 4 (the anti-mud polycarboxylate water-reducing agent of the present invention) have a large water reduction rate and good slump retention performance, and their performance is significantly better than that of Comparative Examples 1 to 2 (conventional polycarboxylate water-reducing agent).

[0054] The above are only preferred embodiments of the present invention, and do not limit the patent scope of the present invention. For those skilled in the art, the present invention may have various changes and modifications. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the patent protection scope of the present invention.

Claims

1. An anti-mud type polycarboxylate water reducer, characterized in that: The raw materials for preparing the anti-mud polycarboxylate water-reducing agent include, by mole percentage, 15% to 25% of unsaturated polyether macromonomer, 60% to 80% of acrylic acid, 1% to 10% of unsaturated phosphite amphoteric monomer, 0.5% to 5% of initiator, 0.01% to 0.5% of chain transfer agent, and the balance is water.

2. The anti-mud type polycarboxylate water reducer according to claim 1, characterized in that: The structure of the unsaturated phosphite amphoteric monomer is shown in formula (I): (I).

3. The anti-mud type polycarboxylate water reducer according to claim 1, characterized in that: The molecular weight of the unsaturated polyether macromonomer is 1000-3000.

4. The anti-mud type polycarboxylate water reducer according to claim 1, characterized in that: The unsaturated polyether macromonomer includes at least one of allyl polyoxyethylene ether, isobutylene alcohol polyoxyethylene ether and isopentyl polyoxyethylene ether.

5. The anti-mud type polycarboxylate water reducer according to claim 1, characterized in that: The initiator includes at least one of hydrogen peroxide, ammonium persulfate or potassium persulfate.

6. The anti-mud type polycarboxylate water reducer according to claim 1, characterized in that: The chain transfer agent is selected from at least one of mercaptopropionic acid, thioglycolic acid, sodium methyl methacrylate sulfonate or sodium propylene sulfonate.

7. The anti-mud type polycarboxylate water reducer according to claim 1, characterized in that: The chemical structural formula of the anti-mud polycarboxylate water reducer is as shown in formula (II): (II), Wherein, R1 is -H or -CH3; R2 is -CH2- or -CH2CH2-; y, z, m, and n are all non-zero integers.

8. A method for preparing an anti-mud polycarboxylate water-reducing agent, characterized in that: The following steps are involved: S1: copolymerizing the unsaturated polyether macromonomer, acrylic acid, unsaturated phosphite amphoteric monomer, initiator and chain transfer agent with water to obtain a copolymer solution; S2: Cooling the copolymer solution, and then adjusting the pH value with an alkaline substance to obtain a clear solution, which is the anti-mud polycarboxylate water-reducing agent.

9. The method for preparing the anti-mud type polycarboxylate water-reducing agent according to claim 8, characterized in that: The copolymerization reaction is carried out at 50° C. to 70° C. for 3 hours to 5 hours.

10. The method for preparing the anti-mud type polycarboxylate water-reducing agent according to claim 8, characterized in that: The cooling is to cool the temperature to below 40°C.

Citation Information

Patent Citations

  • Anti-mud amphoteric polycarboxylate superplasticizer and preparation method thereof

    CN111848880A

  • Phosphonic acid-based monomer and preparation method thereof

    CN116063345A

  • High-adaptability amphoteric phosphate water reducer and preparation method thereof

    CN116478341A