Modified phenolic resin and preparation method thereof
Through chemical modification and physical composite technology, the thermal stability and ablation resistance of phenolic resins are improved, and the problem of easy loss of traditional phenolic resins at high temperatures is solved, and the carbon residue rate and mechanical properties are achieved, which is expanded. Application scope.
Patent Information
- Application Number
- CN202411419060.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-12
- Publication Date
- 2024-11-08
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Traditional phenolic resins are prone to holes and cracks during high-temperature ablation, resulting in rapid material loss, and their heat resistance and carbon residual rate are low, which cannot meet the high requirements of modern materials for corrosion resistance and burning performance.
Using chemical modification and physical composite technology, the blending reaction is reduced and the carbon content is increased by introducing 3-bromopropyne, sodium hydroxide and N,N-dimethylformamide into phenolic resin. , and at the same time, carbon fiber and nano-silicon powder are combined on the surface to form a dense protective layer to improve thermal stability and bond strength.
It significantly improves the thermal stability, ablation resistance and viscosity characteristics of the phenolic resin, enhances its carbon residue and mechanical properties at high temperatures, extends the service life of the material and expands the application field.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of polymer compound modification, and in particular to a modified phenolic resin and a preparation method thereof. Background Art
[0002] Phenolic resin is formed by the polycondensation of phenol and formaldehyde under the action of acidic or alkaline catalysts. It has a history of about 100 years and is one of the most widely used thermosetting resins. As the earliest industrialized synthetic resin, it is often used in construction, chemical industry production, military and other fields because of the easy availability of raw materials, convenient synthesis, and the advantages of heat resistance, corrosion resistance, flame retardancy, low smoke emission during combustion, and ablation resistance after curing. Phenolic resin can be mixed with inorganic or organic fillers to make molding compounds to improve strength, can also be impregnated with fabrics, and can also be foamed, and the product size is stable.
[0003] Phenolic resin has good mechanical properties and heat resistance, but with the rapid development of space technology, higher requirements are placed on the heat resistance and ablation resistance of the resin matrix of corrosion-resistant materials. High residual carbon phenolic resin is an excellent ablation-resistant material. Since the 1960s, it has been used as an instantaneous high-temperature and ablation-resistant material for high-speed aircraft abroad. However, due to the limitations of the molecular structure, the residual carbon rate of traditional phenolic resin is relatively low, only 40-50%. During the high-temperature ablation process, it is severely degraded and easily produces more holes and cracks in the material, causing the material to be lost very quickly. Therefore, improving the heat resistance and residual carbon rate of the resin plays a key role in improving the performance of phenolic resin-based composite materials. Summary of the invention
[0004] The purpose of the present application is to provide a modified phenolic resin, which has the advantages of high carbon residue rate, good thermal stability, high temperature ablation resistance, good mechanical properties and excellent surface wettability.
[0005] Another object of the present application is to provide a method for preparing a modified phenolic resin, which can be simple and convenient.
[0006] In order to solve the above technical problems, the technical solution adopted in this application is: In one aspect, the present application provides a modified phenolic resin, wherein the raw materials include the following components in parts by weight: 80-100 parts of phenolic resin, 8-15 parts of 3-bromopropyne, 3-5 parts of phase transfer catalyst, 2-5 parts of sodium hydroxide, 200-500 parts of N,N-dimethylformamide, 30-50 parts of carbon fiber, 50-100 parts of silicon powder and 5-10 parts of surfactant.
[0007] On the other hand, the present application provides a method for preparing a modified phenolic resin, comprising the following steps: S1. Primary modification: Add N,N-dimethylformamide to a reaction kettle, crush the phenolic resin, then add the phenolic resin, phase transfer catalyst and sodium hydroxide to N,N-dimethylformamide, add 3-bromopropyne after uniform dispersion, raise the temperature, and obtain a resin mixture through blending reaction; S2. Secondary modification: adding silicon powder and surfactant to the resin mixture, adding carbon fiber after ultrasonic dispersion, continuing ultrasonic treatment, and finally heating and curing after impurities removal to obtain the modified phenolic resin.
[0008] Compared with the prior art, the embodiments of the present application have at least the following advantages or beneficial effects: 1. This application first uses 3-bromopropyne to chemically modify the phenolic resin under the conditions of sodium hydroxide and N,N-dimethylformamide (DMF) solvent and polyethylene glycol phase transfer catalyst. In the blending reaction, the hydroxyl groups in the phenolic resin structure are etherified, thereby reducing the reactivity of the methylene group, thereby improving the thermal stability of the phenolic resin. At the same time, 3-bromopropyne is grafted into the phenolic resin as a high-carbon raw material to increase its carbon content to improve the ablation resistance. In addition, the chemical modification process introduces side chains into the phenolic resin structure, reduces the curing crosslinking density of the phenolic resin, thereby improving the viscosity of the phenolic resin, improving the toughness of the phenolic resin, and solving the problems of brittleness and easy cracking of ordinary phenolic resin.
[0009] 2, the present application is in the phenolic resin surface composite carbon fiber after chemical modification, greatly improves the carbon content in the whole phenolic resin composite, and adds nanometer grade silicon powder in the composite process, silicon powder can be used as the binding agent between phenolic resin and carbon fiber on the one hand, improves the bonding effect of carbon fiber on the phenolic resin surface, silicon powder can also have stronger bonding strength under high temperature ablation, for the ablation resistance of phenolic resin at high temperature plays a greater role.On the other hand, the addition of nanoparticles can form physical or chemical crosslinking points in polymer matrix by its own small size effect and surface effect, strengthens the thermal stability of polymer.More importantly, the carbon fiber and silicon powder tightly compounded on the phenolic resin surface can form a dense protective layer on the phenolic resin surface, slow down the pyrolysis of phenolic resin at high temperature, especially reduce the further destruction of carbon monoxide and other volatile components released by this pyrolysis to the resin matrix structure, the resin volatile components are retained in the resin matrix as far as possible, improve its high temperature stability.In addition, physical composite modification forms nano protrusions on phenolic resin and carbon fiber surface, improves its surface wettability and surface energy, changes the external interface binding of phenolic resin.
[0010] In summary, the present application adopts the methods of chemical structure modification and physical composite modification to perform dual modification on phenolic resin, thereby increasing the carbon content of phenolic resin and its residual carbon rate at high temperature, showing excellent thermal stability and ablation resistance, and improving the viscosity characteristics of the resin, increasing the toughness of the phenolic resin, greatly increasing the roughness of the phenolic resin surface and improving the interface wettability, thereby further optimizing the interface properties of the composite material and expanding the application field of phenolic resin. DETAILED DESCRIPTION
[0011] In order to make the purpose, technical scheme and advantages of the embodiments of the present application clearer, the technical scheme in the embodiments of the present application will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to the conventional conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0012] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present application will be described in detail below with reference to specific embodiments.
[0013] A modified phenolic resin, wherein the raw materials include the following components in parts by weight: 80-100 parts of phenolic resin, 8-15 parts of 3-bromopropyne, 3-5 parts of phase transfer catalyst, 2-5 parts of sodium hydroxide, 200-500 parts of N,N-dimethylformamide, 30-50 parts of carbon fiber, 50-100 parts of silicon powder and 5-10 parts of surfactant.
[0014] In some embodiments of the present application, the phase transfer catalyst is polyethylene glycol or tetrabutylammonium bromide; the phase transfer catalyst can help reactants transfer from one phase to another phase where the reaction can occur, thereby accelerating the reaction rate of the heterogeneous system. Sodium hydroxide provides an alkaline environment to promote the modification reaction.
[0015] The above-mentioned surfactant is Tween-40, sodium dodecylbenzene sulfonate, nonylphenol polyoxyethylene ether or castor oil polyoxyethylene ether; the nano silicon powder of the present application is in an energy unstable state because of its large specific surface area and surface energy, so it is easy to agglomerate and cause the particles to increase, thus causing the nano powder to agglomerate. The present application adds a surfactant, whose molecular structure is amphiphilic, with one end being a hydrophilic group and the other end being a hydrophobic group. This special structure enables the surfactant to form a monomolecular film on the surface of its solution, or form micelles in the solution, enhance the dispersibility of the solution, make the nano silicon powder particles evenly dispersed in the liquid, and improve the agglomeration problem of the nano particles in combination with ultrasonic treatment; in addition, the surfactant can also reduce the surface energy of the carbon fiber surface and improve the wettability of the entire phenolic resin.
[0016] In some embodiments of the present application, the silicon powder is nano silicon powder with a size of 30-80nm; the length of the carbon fiber is 1-5mm. Nano silicon powder refers to ultrafine silicon particles with a particle size in the range of 1-100nm. Nanoparticles have unique surface effects, small size effects, quantum effects, and macroscopic quantum tunneling effects. When modified, these characteristics enable nanoparticles to form physical or chemical crosslinking points in the polymer matrix, enhancing the thermal stability of the polymer. At the same time, nano-scale silicon powder can more easily enter between the carbon fiber and the phenolic resin for bonding between the two. The chopped carbon fiber is compounded on the surface of the phenolic resin to reduce the porosity and reduce the self-volatility of the phenolic resin at high temperatures.
[0017] A method for preparing a modified phenolic resin comprises the following steps: S1. One-time modification: Add N,N-dimethylformamide to the reactor, crush the phenolic resin, then add the phenolic resin, phase transfer catalyst and sodium hydroxide to N,N-dimethylformamide, add 3-bromopropyne after uniform dispersion, heat up, and obtain a resin mixture through blending reaction; This application first uses 3-bromopropyne to chemically modify the phenolic resin under the conditions of sodium hydroxide and N,N-dimethylformamide solvent and polyethylene glycol phase transfer catalyst. In the blending reaction, the hydroxyl groups in the phenolic resin structure are etherified, thereby reducing the reaction activity of the methylene group, thereby improving the thermal stability of the phenolic resin. At the same time, 3-bromopropyne is grafted into the phenolic resin as a high-carbon raw material to increase its carbon content to improve the ablation resistance. In addition, the chemical modification process introduces side chains into the phenolic resin structure, reduces the curing crosslinking density of the phenolic resin, thereby improving the viscosity of the phenolic resin (1200-3000mPa·s), improving the toughness of the phenolic resin, and solving the problems of brittleness and easy cracking of ordinary phenolic resin.
[0018] S2, secondary modification: add silicon powder and surfactant to the resin mixture, add carbon fiber after ultrasonic dispersion, continue ultrasonic treatment, and finally heat and solidify after impurities are removed to obtain the modified phenolic resin. The present application composites carbon fiber on the surface of the chemically modified phenolic resin, greatly improving the carbon content in the entire phenolic resin composite, and adding nano-scale silicon powder during the composite process. On the one hand, silicon powder can be used as a binder between phenolic resin and carbon fiber to improve the bonding effect of carbon fiber on the surface of phenolic resin. Even under high-temperature ablation, silicon powder can have a strong bonding strength, which plays a greater role in the ablation resistance of phenolic resin at high temperatures. On the other hand, the addition of nanoparticles can form physical or chemical crosslinking points in the polymer matrix by its own small size effect and surface effect, enhancing the thermal stability of the polymer. More importantly, the carbon fiber and silicon powder tightly compounded on the surface of the phenolic resin can form a dense protective layer on the surface of the phenolic resin, slowing down the pyrolysis of the phenolic resin at high temperatures, and reducing the further damage of the carbon monoxide and other volatile components released by the pyrolysis to the resin matrix structure, and the resin volatile components are retained in the resin matrix as much as possible to improve its high-temperature stability. In addition, physical composite modification enables nano-silicon powder to form nano-protrusions on the surface of phenolic resin and carbon fiber, which can improve their surface wettability and surface energy and change the interface bonding of phenolic resin to the outside.
[0019] In some embodiments of the present application, the stirring speed of the dispersion in the above step S1 is 80-120 r / min, and the stirring time is 20-40 min.
[0020] In some embodiments of the present application, the temperature after heating in the above step S1 is 70-90° C., the stirring speed of the blending reaction is 50-60 r / min, and the reaction time is 80-120 min.
[0021] In some embodiments of the present application, the temperature of ultrasonic dispersion after adding silicon powder and surfactant in the above step S2 is 55-70°C, and the ultrasonic time is 1-3h; the ultrasonic time after adding carbon fiber is 0.5-1h. Ultrasonic dispersion is mainly used to disperse nanoparticles in the mixture to prevent them from agglomerating and affecting the effect.
[0022] In some embodiments of the present application, the heating and curing in the secondary modification in the above step S2 adopts step-by-step temperature curing.
[0023] In some embodiments of the present application, the temperature gradient and holding time of the above-mentioned step-heating curing are specifically: 50-55°C, 3-4h; 70-75°C, 1h; 120-125°C, 1h; 150-160°C, 1h; 170°C, 1h, and then cooled to room temperature. Step-heating curing can promote the cross-linking of polymers during the curing process, increase the cohesive strength of phenolic resin, and thus improve the strength of the resin; at the same time, after gradient heating curing, the viscosity of silicon powder increases, which can make the phenolic resin / nano silicon powder / carbon fiber composite structure more stable.
[0024] In some embodiments of the present application, the gradient heating rate of the above-mentioned heating curing is 5°C / min.
[0025] The features and performance of the present application are further described in detail below in conjunction with the embodiments.
[0026] Example 1 A modified phenolic resin is prepared by the following method: S1. Prepare raw materials: 100 g phenolic resin, 12 g 3-bromopropyne, 4 g phase transfer catalyst (polyethylene glycol), 5 g sodium hydroxide, 500 g N,N-dimethylformamide, 40 g carbon fiber, 80 g silicon powder and 8 g surfactant (Tween-40); S2, adding solvent N, N-dimethylformamide to the reactor, crushing the phenolic resin into powder, then adding the phenolic resin, polyethylene glycol and sodium hydroxide to the N, N-dimethylformamide, stirring at a speed of 100r / min for 30min, dispersing the raw materials evenly in the solvent, then adding 3-bromopropyne while stirring, heating to 75°C, adjusting the stirring speed to 60r / min, stirring and blending for 120min to obtain a resin mixture; S3, the above resin mixture is cooled to room temperature, and then Tween-40 and nano-silicon powder (30-50nm) are added to the resin mixture, ultrasonically dispersed in a water bath at 60°C for 2h, and then carbon fiber (length 1-5mm) is added, and ultrasonicated for 0.5h; after impurity removal, the composite material is sent to an oven, and the heating rate is set to 5°C / min, and stage heating curing is performed (heating from room temperature to 50°C, keeping warm for 3.5h, heating to 75°C, keeping warm for 1h, heating to 120°C, keeping warm for 1h, heating to 150°C, keeping warm for 1h, heating to 170°C, keeping warm for 1h), and then cold-cut to room temperature to obtain the modified phenolic resin of this embodiment.
[0027] Example 2 A modified phenolic resin is prepared by the following method: S1. Prepare raw materials: 90g phenolic resin, 10g 3-bromopropyne, 4g phase transfer catalyst (polyethylene glycol), 5g sodium hydroxide, 400g N,N-dimethylformamide, 30g carbon fiber, 50g silicon powder and 10g surfactant (Tween-40); S2, adding solvent N, N-dimethylformamide to a reactor, crushing the phenolic resin into powder, then adding the phenolic resin, polyethylene glycol and sodium hydroxide to N, N-dimethylformamide, stirring at a speed of 110r / min for 30min, dispersing the raw materials evenly in the solvent, then adding 3-bromopropyne while stirring, heating to 80°C, adjusting the stirring speed to 60r / min, stirring and blending for 100min to obtain a resin mixture; S3, the above resin mixture is cooled to room temperature, and then Tween-40 and nano-silicon powder (30-50nm) are added to the resin mixture, ultrasonically dispersed in a water bath at 65°C for 3h, and then carbon fiber (length 1-5mm) is added, and ultrasonicated for 0.5h; after impurity removal, the composite material is sent to an oven, and the heating rate is set to 5°C / min, and stage heating curing is performed (heating from room temperature to 50°C, keeping warm for 4h, heating to 75°C, keeping warm for 1h, heating to 120°C, keeping warm for 1h, heating to 150°C, keeping warm for 1h, heating to 170°C, keeping warm for 1h), and the modified phenolic resin of the present embodiment is obtained after cooling to room temperature.
[0028] Example 3 A modified phenolic resin is prepared by the following method: S1. Prepare raw materials: 90g phenolic resin, 15g 3-bromopropyne, 3g phase transfer catalyst (tetrabutylammonium bromide), 3g sodium hydroxide, 300g N,N-dimethylformamide, 30g carbon fiber, 80g silicon powder and 5g surfactant (castor oil polyoxyethylene ether); S2, adding solvent N, N-dimethylformamide to a reactor, crushing the phenolic resin into powder, then adding the phenolic resin, polyethylene glycol and sodium hydroxide to N, N-dimethylformamide, stirring at a speed of 80r / min for 40min, dispersing the raw materials evenly in the solvent, then adding 3-bromopropyne while stirring, heating to 85°C, adjusting the stirring speed to 60r / min, stirring and blending for 90min to obtain a resin mixture; S3, the above resin mixture is cooled to room temperature, and then Tween-40 and nano-silicon powder (30-50nm) are added to the resin mixture, ultrasonically dispersed in a 60°C water bath for 1.5h, and then carbon fiber (length 1-5mm) is added, and ultrasonicated for 1h; after impurity removal, the composite material is sent to an oven, and the heating rate is set to 5°C / min, and stage heating curing is performed (heating from room temperature to 50°C, keeping warm for 4h, heating to 75°C, keeping warm for 1h, heating to 120°C, keeping warm for 1h, heating to 155°C, keeping warm for 1h, heating to 170°C, keeping warm for 1h), and then cold-cut to room temperature to obtain the modified phenolic resin of this embodiment.
[0029] Example 4 A modified phenolic resin is prepared by the following method: S1. Prepare raw materials: 80g phenolic resin, 15g 3-bromopropyne, 4g phase transfer catalyst (polyethylene glycol), 3g sodium hydroxide, 350g N,N-dimethylformamide, 35g carbon fiber, 100g silicon powder and 7g surfactant (nonylphenol polyoxyethylene ether); S2, adding solvent N, N-dimethylformamide to the reactor, crushing the phenolic resin into powder, then adding the phenolic resin, polyethylene glycol and sodium hydroxide to the N, N-dimethylformamide, stirring at a speed of 80r / min for 25min, dispersing the raw materials evenly in the solvent, then adding 3-bromopropyne while stirring, heating to 85°C, adjusting the stirring speed to 60r / min, stirring and blending for 80min to obtain a resin mixture; S3, the above resin mixture is cooled to room temperature, and then Tween-40 and nano-silicon powder (30-80nm) are added to the resin mixture, ultrasonically dispersed in a 70°C water bath for 1.5h, and then carbon fiber (length 1-5mm) is added, and ultrasonicated for 0.5h; after impurity removal, the composite material is sent to an oven, and the heating rate is set to 5°C / min, and stage heating curing is performed (heating from room temperature to 55°C, keeping warm for 4h, heating to 75°C, keeping warm for 1h, heating to 125°C, keeping warm for 1h, heating to 155°C, keeping warm for 1h, heating to 170°C, keeping warm for 1h), and the modified phenolic resin of the present embodiment is obtained after cooling to room temperature.
[0030] Example 5 A modified phenolic resin is prepared by the following method: S1. Prepare raw materials: 100g phenolic resin, 10g 3-bromopropyne, 4g phase transfer catalyst (polyethylene glycol), 5g sodium hydroxide, 450g N,N-dimethylformamide, 30g carbon fiber, 90g silicon powder and 8g surfactant (sodium dodecylbenzene sulfonate); S2, adding solvent N, N-dimethylformamide to a reactor, crushing the phenolic resin into powder, then adding the phenolic resin, polyethylene glycol and sodium hydroxide to N, N-dimethylformamide, stirring at a speed of 100 r / min for 20 min, dispersing the raw materials evenly in the solvent, then adding 3-bromopropyne while stirring, heating to 90 ° C, adjusting the stirring speed to 60 r / min, stirring and blending for 100 min to obtain a resin mixture; S3, the above resin mixture is cooled to room temperature, and then Tween-40 and nano-silicon powder (30-80nm) are added to the resin mixture, ultrasonically dispersed in a 70°C water bath for 1.5h, and then carbon fiber (length 1-5mm) is added, and ultrasonicated for 0.5h; after impurity removal, the composite material is sent to an oven, and the heating rate is set to 5°C / min, and stage heating curing is performed (heating from room temperature to 50°C, keeping warm for 4h, heating to 70°C, keeping warm for 1h, heating to 125°C, keeping warm for 1h, heating to 160°C, keeping warm for 1h, heating to 170°C, keeping warm for 1h), and the modified phenolic resin of the present embodiment is obtained after cooling to room temperature.
[0031] Comparative Example 1 The difference between this comparative example and Example 1 is that the resin mixture obtained in step S2 is cured after impurities are removed, specifically: S1. Prepare raw materials: 100 g phenolic resin, 12 g 3-bromopropyne, 4 g phase transfer catalyst (polyethylene glycol), 5 g sodium hydroxide, 500 g N,N-dimethylformamide; S2, adding solvent N, N-dimethylformamide to the reactor, crushing the phenolic resin into powder, then adding the phenolic resin, polyethylene glycol and sodium hydroxide to the N, N-dimethylformamide, stirring at a speed of 100r / min for 30min, dispersing the raw materials evenly in the solvent, then adding 3-bromopropyne while stirring, heating to 75°C, adjusting the stirring speed to 60r / min, stirring and blending for 120min to obtain a resin mixture; S3. After removing impurities from the above resin mixture, it was sent into an oven, and the temperature rate was set to 5°C / min and the insulation time of each stage temperature was set for heating and curing (heating from room temperature to 50°C, insulation for 3.5h, heating to 75°C, insulation for 1h, heating to 120°C, insulation for 1h, heating to 150°C, insulation for 1h, heating to 170°C, insulation for 1h), and then cooled to room temperature to obtain the modified phenolic resin of this comparative example.
[0032] Comparative Example 2 The difference between this comparative example and Example 1 is that the phenolic resin is not modified with 3-bromopropyne, specifically: S1. Prepare raw materials: 100 g phenolic resin, 500 g N,N-dimethylformamide, 40 g carbon fiber, 80 g silicon powder and 8 g surfactant (Tween-40); S2, adding solvent N,N-dimethylformamide into a reaction kettle, crushing the phenolic resin into powder, then adding the phenolic resin to the N,N-dimethylformamide, stirring at a speed of 100 r / min for 30 min to evenly disperse the phenolic resin to obtain a resin mixture; S3, add Tween-40 and nano-silicon powder (30-50nm) to the above resin mixture, ultrasonically disperse in a water bath at 60°C for 2h, then add carbon fiber (length 1-5mm), and ultrasonically disperse for 0.5h; after impurity removal, send the composite material into an oven, set the heating rate to 5°C / min, and perform stage heating and curing (heating from room temperature to 50°C, keeping warm for 3.5h, heating to 75°C, keeping warm for 1h, heating to 120°C, keeping warm for 1h, heating to 150°C, keeping warm for 1h, heating to 170°C, keeping warm for 1h), and obtain the modified phenolic resin of the present embodiment after cooling to room temperature.
[0033] Comparative Example 3 The difference between this comparative example and Example 1 is that in this comparative example, nano-scale silicon powder is not added when the resin mixture is composited with carbon fiber, specifically: S1. Prepare raw materials: 100 g phenolic resin, 12 g 3-bromopropyne, 4 g phase transfer catalyst (polyethylene glycol), 5 g sodium hydroxide, 500 g N,N-dimethylformamide, 40 g carbon fiber and 8 g surfactant (Tween-40); S2, adding solvent N, N-dimethylformamide to the reactor, crushing the phenolic resin into powder, then adding the phenolic resin, polyethylene glycol and sodium hydroxide to the N, N-dimethylformamide, stirring at a speed of 100r / min for 30min, dispersing the raw materials evenly in the solvent, then adding 3-bromopropyne while stirring, heating to 75°C, adjusting the stirring speed to 60r / min, stirring and blending for 120min to obtain a resin mixture; S3, the above resin mixture is cooled to room temperature, and then Tween-40 is added to the resin mixture, ultrasonically dispersed in a water bath at 60°C for 2h, and then carbon fiber (length 1-5mm) is added, and ultrasonicated for 0.5h; after impurity removal, the composite material is sent to an oven, and the heating rate is set to 5°C / min, and stage heating curing is performed (heating from room temperature to 50°C, keeping warm for 3.5h, heating to 75°C, keeping warm for 1h, heating to 120°C, keeping warm for 1h, heating to 150°C, keeping warm for 1h, heating to 170°C, keeping warm for 1h), and then cold-cut to room temperature to obtain the modified phenolic resin of this embodiment.
[0034] Comparative Example 4 The difference between this comparative example and comparative example 3 is that the amount of carbon fiber added in this comparative example is 120 g.
[0035] Comparative Example 5 The difference between this comparative example and Example 1 is that no carbon fiber is added in this comparative example. The specific preparation method is: S1. Prepare raw materials: 100 g phenolic resin, 12 g 3-bromopropyne, 4 g phase transfer catalyst (polyethylene glycol), 5 g sodium hydroxide, 500 g N,N-dimethylformamide, 80 g silicon powder and 8 g surfactant (Tween-40); S2, adding solvent N, N-dimethylformamide to the reactor, crushing the phenolic resin into powder, then adding the phenolic resin, polyethylene glycol and sodium hydroxide to the N, N-dimethylformamide, stirring at a speed of 100r / min for 30min, dispersing the raw materials evenly in the solvent, then adding 3-bromopropyne while stirring, heating to 75°C, adjusting the stirring speed to 60r / min, stirring and blending for 120min to obtain a resin mixture; S3, the above resin mixture is cooled to room temperature, and then Tween-40 and nano-silicon powder (30-50nm) are added to the resin mixture, and ultrasonically dispersed in a 60°C water bath for 2h; after impurity removal, the composite material is sent to an oven, and the heating rate is set to 5°C / min, and stage heating curing is performed (heating from room temperature to 50°C, keeping warm for 3.5h, heating to 75°C, keeping warm for 1h, heating to 120°C, keeping warm for 1h, heating to 150°C, keeping warm for 1h, heating to 170°C, keeping warm for 1h), and then cooled to room temperature to obtain the modified phenolic resin of this embodiment.
[0036] Experimental example 1. The modified phenolic resins prepared in Examples 1-5 and Comparative Examples 1-5 were subjected to thermogravimetric analysis at a heating rate of 10°C / min, and the untreated phenolic resin was used as a blank control. The pyrolysis point temperature and pyrolysis peak temperature of the phenolic resins in each experimental group and the control group are shown in Table 1.
[0037] Table 1
[0038] As can be seen from Table 1, compared with the blank control group, the thermal decomposition temperatures of the modified phenolic resins prepared in Examples 1-5 and Comparative Examples 1-5 are significantly increased, indicating that both modification steps can effectively improve the thermal stability of the phenolic resin. Analysis of Comparative Examples 1-5 shows that the chemical structure of the phenolic resin modified by blending 3-bromopropyne is more effective in improving thermal stability than directly compounding high-carbon raw material carbon fiber and silicon powder on the surface of the phenolic resin.
[0039] 2. The modified phenolic resins prepared in Examples 1-5 and Comparative Examples 1-5 were heated to 700°C and 900°C at a heating rate of 10°C / min in a carbonization furnace under a nitrogen atmosphere to perform a performance test on the residual carbon rate. Untreated phenolic resin was used as a blank control. The results are shown in Table 2.
[0040] Table 2
[0041] As can be seen from Table 2, compared with the untreated phenolic resin blank control group, the residual carbon rate of the modified phenolic resin in Examples 1-5 and Comparative Examples 1-5 is significantly improved, indicating that the chemical structure of the phenolic resin modified by blending 3-bromopropyne and the direct physical compounding of high-carbon raw materials carbon fiber and silicon powder on the surface of the phenolic resin can increase the carbon content of the phenolic resin, thereby improving its residual carbon rate at high temperature.
[0042] It is also worth noting that compared with the residual carbon rate of Example 3 and Example 4, although the proportion of carbon fiber is increased in Example 4, its residual carbon rate does not change significantly under the condition of no nano-silicon powder, indicating that the proportion of carbon fiber added in Example 3 may have reached the best, or in the absence of silicon powder bonding, even if the proportion of carbon fiber is increased, it cannot be better composited with phenolic resin, indicating that nano-silicon powder plays an indispensable connecting role in the composite process of carbon fiber and phenolic resin.
[0043] 3. The tensile strength and full strength tests were performed on the products of Example 1, Comparative Examples 1-5 and the blank control group, as shown in Table 3.
[0044] Table 3
[0045] As can be seen from Table 3, compared with the phenolic resin in the blank control group, the modified phenolic resin in Example 1 has obvious improvements in mechanical properties, indicating that whether introducing side chains into the resin structure by chemical modification or compounding other mechanical modification molecules on the surface can increase the viscosity of the phenolic resin, thereby improving the toughness of the phenolic resin, increasing the tensile strength and flexural strength, and solving the problem of easy cracking of traditional phenolic resin.
[0046] Compared with Example 1, the tensile strength and flexural strength of Comparative Examples 1-5 are slightly decreased, which further proves that the primary modification and secondary modification of the phenolic resin have an effect on its mechanical properties, especially the mechanical properties of Comparative Examples 1, 3 and 4 are more decreased. It can be seen that the compounding of carbon fiber and silicon powder on phenolic resin has a greater effect on the toughness modification of the resin.
[0047] In summary, the modified phenolic resin and preparation method thereof according to the embodiment of the present application have the following advantages: 1. This application first uses 3-bromopropyne to chemically modify the phenolic resin under the conditions of sodium hydroxide and N,N-dimethylformamide (DMF) solvent and polyethylene glycol phase transfer catalyst. In the blending reaction, the hydroxyl groups in the phenolic resin structure are etherified, thereby reducing the reactivity of the methylene group, thereby improving the thermal stability of the phenolic resin. At the same time, 3-bromopropyne is grafted into the phenolic resin as a high-carbon raw material to increase its carbon content to improve the ablation resistance. In addition, the chemical modification process introduces side chains into the phenolic resin structure, reduces the curing crosslinking density of the phenolic resin, thereby improving the viscosity characteristics of the phenolic resin, improving the toughness of the phenolic resin, and solving the problems of brittleness and easy cracking of ordinary phenolic resin.
[0048] 2, the present application is in the phenolic resin surface composite carbon fiber after chemical modification, greatly improves the carbon content in the whole phenolic resin composite, and adds nanometer grade silicon powder in the composite process, silicon powder can be used as the binding agent between phenolic resin and carbon fiber on the one hand, improves the bonding effect of carbon fiber on the phenolic resin surface, even silicon powder can also have stronger bonding strength under high temperature ablation, for the ablation resistance of phenolic resin at high temperature plays a greater role.On the other hand, the small size effect and surface effect of the addition of nanoparticles especially itself can form physical or chemical crosslinking points in polymer matrix, strengthen the thermal stability of polymer.More importantly, the carbon fiber and silicon powder tightly compounded on the phenolic resin surface can form a dense protective layer on the phenolic resin surface, slow down the pyrolysis of phenolic resin at high temperature, especially reduce the further destruction of carbon monoxide and other volatile components released by this pyrolysis to the resin matrix structure, the resin volatile components are retained in the resin matrix as far as possible, improve its high temperature stability.In addition, physical composite modification forms nano protrusions on phenolic resin and carbon fiber surface, improves its surface wettability and surface energy, changes the external interface binding of phenolic resin.
[0049] In summary, the present application adopts the methods of chemical structure modification and physical composite modification to perform dual modification on phenolic resin, thereby increasing the carbon content of phenolic resin and its residual carbon rate at high temperature, showing excellent thermal stability and ablation resistance, and improving the viscosity characteristics of the resin, increasing the toughness of the phenolic resin, greatly increasing the roughness of the phenolic resin surface and improving the interface wettability, thereby further optimizing the interface properties of the composite material and expanding the application field of phenolic resin.
[0050] The embodiments described above are part of the embodiments of the present application, rather than all of the embodiments. The detailed description of the embodiments of the present application is not intended to limit the scope of the present application for protection, but merely represents the selected embodiments of the present application. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work belong to the scope of protection of the present application.
Claims
1. A modified phenolic resin, characterized in that: The raw materials include the following components by weight: 80-100 parts of phenolic resin, 8-15 parts of 3-bromopropyne, 3-5 parts of phase transfer catalyst, 2-5 parts of sodium hydroxide, 200-500 parts of N,N-dimethylformamide, 30-50 parts of carbon fiber, 50-100 parts of silicon powder and 5-10 parts of surfactant.
2. A modified phenolic resin according to claim 1, characterized in that: The phase transfer catalyst is polyethylene glycol or tetrabutylammonium bromide; the surfactant is Tween-40, sodium dodecylbenzene sulfonate, nonylphenol polyoxyethylene ether or castor oil polyoxyethylene ether.
3. A modified phenolic resin according to claim 1, characterized in that: The silicon powder is nano silicon powder with a size of 30-80nm; the length of the carbon fiber is 1-5mm.
4. A method for preparing a modified phenolic resin as claimed in any one of claims 1 to 3, characterized in that: The following steps are involved: S1. Primary modification: Add N,N-dimethylformamide to a reaction kettle, crush the phenolic resin, then add the phenolic resin, phase transfer catalyst and sodium hydroxide to N,N-dimethylformamide, add 3-bromopropyne after uniform dispersion, raise the temperature, and obtain a resin mixture through blending reaction; S2. Secondary modification: adding silicon powder and surfactant to the resin mixture, adding carbon fiber after ultrasonic dispersion, continuing ultrasonic treatment, and finally heating and curing after impurities removal to obtain the modified phenolic resin.
5. The method for preparing a modified phenolic resin according to claim 4, characterized in that: The stirring speed of the dispersion in the first modification in step S1 is 80-120 r / min, and the stirring time is 20-40 min.
6. The method for preparing a modified phenolic resin according to claim 4, characterized in that: The temperature after the first modification and heating in step S1 is 70-90° C., the stirring speed of the blending reaction is 50-60 r / min, and the reaction time is 80-120 min.
7. The method for preparing a modified phenolic resin according to claim 4, characterized in that: In the secondary modification of step S2, the temperature of ultrasonic dispersion after adding silicon powder and surfactant is 55-70° C., and the ultrasonic time is 1-3 h; and the ultrasonic time after adding carbon fiber is 0.5-1 h.
8. The method for preparing a modified phenolic resin according to claim 4, characterized in that: The heating and curing in the secondary modification of step S2 adopts step-by-step temperature rise curing.
9. The method for preparing a modified phenolic resin according to claim 8, characterized in that: The temperature gradient and holding time of the step-by-step curing are specifically as follows: 50-55°C, 3-4h; 70-75°C, 1h; 120-125°C, 1h; 150-160°C, 1h; 170°C, 1h, and then cooled to room temperature.
10. The method for preparing a modified phenolic resin according to claim 9, characterized in that: The gradient heating rate of the heating curing is 5°C / min.
Citation Information
Cited By
Flame-retardant wave-absorbing material based on expanded polystyrene and preparation method thereof
CN119910975A
A flame-retardant wave-absorbing material based on expanded polystyrene and its preparation method
CN119910975B