Soft aliphatic polyurethane resin with high wear resistance and high folding resistance and preparation method thereof
By combining polycarbonate thiol polyol and aliphatic diisocyanate, the ratio of carbonate groups and sulfide groups is adjusted, and the problem of aliphatic polyurethane resins is solved, and the wear resistance and fold resistance of aliphatic polyurethane resins is achieved is achieved. , high folding resistance and yellowing resistance to soft aliphatic polyurethane resin preparation improves the performance of synthetic leather and simplifies the production process.
Patent Information
- Application Number
- CN202411118952.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-11-08
AI Technical Summary
When aliphatic polyurethane resin improves wear resistance, its cold and fold resistance decreases, and its color is easily turned yellow due to light, making it difficult to meet the wear resistance, fold resistance and yellowing requirements of soft resins at the same time.
Using the combination of polycarbonate thiol polyol and aliphatic diisocyanate and other materials, the ratio of carbonate groups and sulfide groups is adjusted to increase the intermolecular action force and flexibility, and high wear resistance is prepared. Folded soft, high wear and high fold resistance aliphatic polyurethane resin, and reduces production costs through specific preparation methods.
The soft aliphatic polyurethane resin has achieved high wear resistance, high fold resistance and yellowing resistance, which improves the overall performance of synthetic leather, simplifies the preparation process, and facilitates industrial production.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of polyurethane resins, and in particular to a soft, highly wear-resistant and folding-resistant aliphatic polyurethane resin and a preparation method thereof. Background Art
[0002] Polyurethane resin has excellent softness and high strength, and is widely used in various fields. Especially in the field of synthetic leather, polyurethane resin for leather has always been in a leading position in the field of leather resin due to its varied styles and wide applicability.
[0003] Polyurethane resins for leather are mainly divided into two categories: aromatic polyurethane resins and aliphatic polyurethane resins. Aromatic polyurethane resins have better mechanical properties than aliphatic polyurethane resins because they contain benzene rings in their molecular structure; however, since the benzene ring structure is connected to the urethane group, it is easy to produce color-developing groups when exposed to light, causing the color to turn yellow when making light-colored products. Aliphatic polyurethane resins have excellent light resistance due to their saturated aliphatic hydrocarbons in their structure, but their mechanical properties are poor, especially the wear resistance of soft resins is poor.
[0004] Generally, aliphatic polyurethane resins are synthesized using polycarbonate polyols to improve wear resistance, but polycarbonate polyols have a disadvantage, which is that they are hard and brittle. While improving wear resistance, their cold resistance and folding resistance are greatly reduced, which has always been a pain point in the industry. To this end, the inventors provide a soft, highly wear-resistant and folding-resistant aliphatic polyurethane resin and a preparation method thereof. Summary of the invention
[0005] In order to solve the above technical problems, the present application provides a soft aliphatic polyurethane resin with high wear resistance and high folding resistance and a preparation method thereof, so that the soft aliphatic polyurethane resin has good wear resistance and folding resistance.
[0006] The soft, highly wear-resistant and folding-resistant aliphatic polyurethane resin provided in the present application is realized by the following scheme: A soft, highly wear-resistant and folding-resistant aliphatic polyurethane resin is prepared from aliphatic diisocyanate, polyol, chain extender, solvent, catalyst, terminator and functional additive; The polyol is a polycarbonate thiol polyol with a number average molecular weight of 1000-3000 and at least one of a polyether polyol and a polyester polyol with a number average molecular weight of 1000-4000; The polycarbonate thiol polyol is made of dithiol, diethyl carbonate, a catalyst and an antioxidant; At least one of the dithiol ethanedithiol, 1,3 propanedithiol, 1,4 butanedithiol, and 1,6 hexanedithiol; The catalyst is at least one of tetrabutyl titanate, tetra-tert-butyl titanate, and dibutyltin dilaurate; The aliphatic diisocyanate is at least one of isophorone diisocyanate, 4,4′-dicyclohexylmethane diisocyanate and hexamethylene diisocyanate; The chain extender is at least one of a diol or a triol having a molecular weight of 61-500 g / mol; The solvent is one or a mixture of two or more of dimethylformamide, methyl ethyl ketone, toluene, ethyl acetate, dimethyl carbonate, and acetone; The catalyst is organic tin and / or organic bismuth; The terminator is at least one of methanol and ethanol; The functional additives include at least one of an antioxidant, an ultraviolet absorber, a stabilizer, an anti-hydrolysis agent, and a flame retardant.
[0007] The soft, highly wear-resistant and fold-resistant aliphatic polyurethane resin polyurethane in the present application contains a large number of carbonate groups in the molecular chain. The carbonate groups have large internal energy and strong intermolecular forces, which increase the wear resistance of the resin; at the same time, the molecular chain contains thioether groups. The thioether atomic radius is large and the molecular chain flexibility is very good, which increases the folding resistance of the molecule. By introducing carbonate groups and thioether groups and adjusting the appropriate ratio of the two, a soft aliphatic polyurethane resin product that is both wear-resistant and fold-resistant can be synthesized.
[0008] Preferably, the preparation method of the polycarbonate thiol polyol is as follows: put dithiol, diethyl carbonate, a catalyst, and an antioxidant into a reactor, raise the temperature of the reactor to 140-145°C, control the outlet temperature at the top of the cooling tube at 65-126°C, gradually raise the temperature of the reactor to 200-205°C at a heating rate of 15-20°C / h, and keep the reaction at 200°C for 2-4h; maintain the vacuum degree of -0.05 to -0.08 MPa for 2-3h; then increase the vacuum degree of the reactor to -0.08 to -0.095 MPa for 2-3h, and take samples for testing to obtain a polycarbonate thiol polyol with a hydroxyl value of 37.3-112mgKOH / g.
[0009] By adopting the above technical solution, polycarbonate thiol polyol can be prepared in batches, thereby reducing the overall production cost.
[0010] Preferably, the total molar amount of active groups in the polyol and chain extender is 0.95-1.10 times the molar amount of isocyanate groups in the aliphatic diisocyanate.
[0011] Preferably, the total molar amount of active groups in the polyol and the molar amount of hydroxyl groups in the chain extender are prepared to be 1:(1.05-2.00).
[0012] By adopting the above technical solution, it can be ensured that the prepared synthetic leather has the advantages of being soft, wear-resistant, fold-resistant and anti-yellowing.
[0013] Preferably, the soft, highly wear-resistant and folding-resistant aliphatic polyurethane resin is made of 4,4′-dicyclohexylmethane diisocyanate, polycarbonate thiol polyol with a number average molecular weight of 2000, polytetramethylene furan diol with a number average molecular weight of 2000, ethylene glycol, dimethyl carbonate, dimethylformamide, stannous octoate, methanol, and triphenyl phosphite.
[0014] Preferably, the soft, highly wear-resistant and folding-resistant aliphatic polyurethane resin is made of isophorone diisocyanate, polycarbonate thiol polyol with a number average molecular weight of 1500, 1,4-butanediol, dimethylformamide, bismuth carboxylate, methanol, and triphenyl phosphite.
[0015] Preferably, the soft, highly wear-resistant and folding-resistant aliphatic polyurethane resin is made of hexamethylene diisocyanate, polycarbonate thiol polyol with a number average molecular weight of 1500, poly(1,6-hexanediol adipate) with a number average molecular weight of 3500, 1,6-hexanediol, methyl ethyl ketone, dimethylformamide, dibutyltin dilaurate, ethanol, and antioxidant 1024.
[0016] Preferably, the soft, highly wear-resistant and folding-resistant aliphatic polyurethane resin is made of 4,4′-dicyclohexylmethane diisocyanate, polycarbonate thiol polyol with a number average molecular weight of 3000, polypropylene oxide diol with a number average molecular weight of 2000, polytetramethylene oxide diol with a number average molecular weight of 3000, polyethylene adipate glycol 1,4-butylene glycol ester diol with a number average molecular weight of 2000, 1,3-propylene glycol, dimethylformamide, toluene, dibutyltin dilaurate, methanol, and triphenyl phosphite.
[0017] Preferably, the soft, highly wear-resistant and folding-resistant aliphatic polyurethane resin is made of isophorone diisocyanate, polycarbonate thiol polyol with a number average molecular weight of 1000, polyethylene adipate 1,2-propylene glycol ester diol with a number average molecular weight of 1500, ethylene glycol, dimethylformamide, methyl ethyl ketone, dibutyl tin dilaurate, methanol, and antioxidant 1010.
[0018] By adopting the above technical solution, it can be ensured that the prepared synthetic leather has the advantages of being soft, wear-resistant, fold-resistant and anti-yellowing.
[0019] The present application provides a method for preparing a soft, highly wear-resistant and highly folding-resistant aliphatic polyurethane resin, which is achieved through the following technical solutions: A method for preparing a soft, highly wear-resistant and folding-resistant aliphatic polyurethane resin comprises the following steps: Step 1, preparation of polycarbonate thiol polyol: put dithiol, diethyl carbonate, catalyst, and antioxidant into a reactor, raise the temperature of the reactor to 140-145°C, control the outlet temperature of the top of the cooling tube at 65-126°C, gradually raise the temperature of the reactor to 200-205°C at a heating rate of 15-20°C / h, and keep the temperature at 200°C for 2-4h; keep the vacuum degree at -0.05 to -0.08 MPa for 2-3h; then increase the vacuum degree of the reactor to -0.08 to -0.095 MPa for 2-3h, and take samples for testing to obtain polycarbonate thiol polyol with a hydroxyl value of 37.3-112mgKOH / g; Step 2: Add polyol, chain extender, solvent accounting for 20-30wt% of the total solvent mass, and functional additive into the reactor, heat to 45-50°C, and stir evenly; add aliphatic diisocyanate, control the kettle temperature at 85-90°C to react for 1-1.5h, add solvent accounting for 20-30wt% of the total solvent mass, control the reaction temperature to 88-92°C to continue the reaction, add the remaining solvent into the reactor as the viscosity increases, add the catalyst until the viscosity reaches 4×103-2×105mPa•s / 25°C, add terminator to react for 30-90min, and unload to obtain a soft, highly wear-resistant and fold-resistant aliphatic polyurethane resin.
[0020] The preparation method provided in this application is relatively simple, has low production difficulty, and is easy to implement industrial production.
[0021] In summary, this application has the following advantages: 1. The synthetic leather prepared by the present application has the advantages of being soft, wear-resistant, fold-resistant, and resistant to yellowing and aging.
[0022] 2. The preparation method provided in this application is relatively simple, with low production difficulty, and is easy to realize industrial production. DETAILED DESCRIPTION
[0023] In order to further understand the present invention, preferred embodiments of the present invention are described below in conjunction with examples and comparative examples.
[0024] Preparation Example 1: Preparation of polycarbonate thiol polyol with a number average molecular weight of 2000: 1671g of 1,4-butanedithiol, 1252g of dimethyl carbonate, 5g of tetrabutyl titanate, and 3g of antioxidant 1010 are put into a reactor, the temperature of the reactor is raised to 140°C, the outlet temperature at the top of the cooling tube is controlled at 65°C, the temperature of the reactor is gradually raised to 200°C at a heating rate of 15°C / h, and the reaction is kept at 200°C for 2h; the vacuum degree is maintained at -0.05 to -0.08 MPa for 2h; the vacuum degree of the reactor is increased to -0.08 to -0.095 MPa for 2h, and a sample test is performed to obtain 0.56mgKOH / g of thiol (the thiol value test method is the same as the hydroxyl value test method), and the polycarbonate thiol polyol with a number average molecular weight of 2000 can be obtained by unloading.
[0025] Preparation Example 2: Preparation of polycarbonate thiol polyol with a number average molecular weight of 1500: 1301g of 1,6-hexanedithiol, 758g of dimethyl carbonate, 4g of dibutyltin dilaurate, and 2g of antioxidant 1010 were put into a reactor, the temperature of the reactor was raised to 140°C, the outlet temperature at the top of the cooling tube was controlled at 65°C, the temperature of the reactor was gradually raised to 200°C at a heating rate of 15°C / h, and the reaction was kept at 200°C for 4h; the vacuum degree was maintained at -0.05 to -0.08 MPa for 3h; the vacuum degree of the reactor was increased to -0.08 to -0.095 MPa for 3h, and the thiol value was obtained by sampling and testing to obtain 74.6mgKOH / g, and the polycarbonate thiol polyol with a number average molecular weight of 1500 was obtained by unloading.
[0026] Preparation Example 3: Preparation of polycarbonate thiol polyol with a number average molecular weight of 1500: 1301g of 1,6-hexanedithiol, 959g of diethyl carbonate, 4g of tetrabutyl titanate, and 3g of antioxidant 1076 are put into a reactor, the temperature of the reactor is raised to 140°C, the outlet temperature at the top of the cooling tube is controlled at 126°C, the temperature of the reactor is gradually raised to 200°C at a heating rate of 15°C / h, and the reaction is kept at 200°C for 4h; the vacuum degree is maintained at -0.05 to -0.08 MPa for 3h; the vacuum degree of the reactor is then increased to -0.08 to -0.095 MPa for 3h, and the thiol value is obtained by sampling and testing to obtain 74.6mgKOH / g, and the polycarbonate thiol polyol with a number average molecular weight of 1500 can be obtained by unloading.
[0027] Preparation Example 4: Preparation of polycarbonate thiol polyol with a number average molecular weight of 3000: 121 g of 1,6-hexanediol, 277 g of diethyl carbonate, 121 g of ethanedithiol, 1.5 g of tetrabutyl titanate, and 1 g of antioxidant 1076 were put into a reactor, the temperature of the reactor was raised to 140°C, the outlet temperature at the top of the cooling tube was controlled at 126°C, the reactor temperature was gradually raised to 200°C at a heating rate of 15°C / h, and the reaction was kept at 200°C for 4h; the vacuum degree was maintained at -0.05 to -0.08 MPa for 3h; the vacuum degree of the reactor was increased to -0.08 to -0.095 MPa for 3h, and the sample test showed a thiol value of 37.3 mgKOH / g. The polycarbonate thiol polyol with a number average molecular weight of 3000 was obtained by unloading.
[0028] Preparation Example 5: Preparation of polycarbonate thiol polyol with a number average molecular weight of 1000: 194.5 g of neopentyl glycol, 166 g of dimethyl carbonate, 50 g of ethanedithiol, 0.02 g of tetra-tert-butyl titanate, and 0.03 g of antioxidant 1076 were put into a reactor, the temperature of the reactor was raised to 140°C, the outlet temperature at the top of the cooling tube was controlled at 65°C, the temperature of the reactor was gradually raised to 200°C at a heating rate of 15°C / h, and the reaction was kept at 200°C for 2h; the vacuum degree was maintained at -0.05 to -0.08 MPa for 2h; the vacuum degree of the reactor was increased to -0.08 to -0.095 MPa for 2h, and the sample test showed a thiol value of 112 mgKOH / g. The polycarbonate thiol polyol with a number average molecular weight of 1000 was obtained by unloading.
[0029] The difference between Preparation Example 6 and Preparation Example 1 is: Preparation of polycarbonate polyol with a number average molecular weight of 2000: 1417.6g of 1,4-butanediol, 1252g of dimethyl carbonate, 5g of tetrabutyl titanate, and 3g of antioxidant 1010 are put into a reactor, the temperature of the reactor is raised to 140°C, the outlet temperature at the top of the cooling tube is controlled at 65°C, the temperature of the reactor is gradually raised to 200°C at a heating rate of 15°C / h, and the reaction is kept at 200°C for 2h; the vacuum degree is maintained at -0.05 to -0.08 MPa for 2h; the vacuum degree of the reactor is increased to -0.08 to -0.095 MPa for 2h, and the sampling test obtains a thiol value of 56mgKOH / g, and the polycarbonate polyol with a number average molecular weight of 2000 can be obtained by unloading.
[0030] The difference between Preparation Example 7 and Preparation Example 2 is: Preparation of polycarbonate polyol with a number average molecular weight of 1500: 1022.8g of 1,6-hexanediol, 758g of dimethyl carbonate, 4g of dibutyltin dilaurate, and 2g of antioxidant 1010 are put into a reactor, the temperature of the reactor is raised to 140°C, the outlet temperature at the top of the cooling tube is controlled at 65°C, the temperature of the reactor is gradually raised to 200°C at a heating rate of 15°C / h, and the reaction is kept at 200°C for 4h; the vacuum degree is maintained at -0.05 to -0.08 MPa for 3h; the vacuum degree of the reactor is then increased to -0.08 to -0.095 MPa for 3h, and the thiol value is obtained by sampling and testing to obtain 74.6mgKOH / g, and the polycarbonate polyol with a number average molecular weight of 1500 can be obtained by unloading.
[0031] The difference between Preparation Example 8 and Preparation Example 3 is: Preparation of polycarbonate polyol with a number average molecular weight of 1500: 1022.8g of 1,6-hexanediol, 959g of diethyl carbonate, 4g of tetrabutyl titanate, and 3g of antioxidant 1076 are put into a reactor, the temperature of the reactor is raised to 140°C, the outlet temperature at the top of the cooling tube is controlled at 126°C, the reactor temperature is gradually raised to 200°C at a heating rate of 15°C / h, and the reaction is kept at 200°C for 4h; the vacuum degree is maintained at -0.05 to -0.08 MPa for 3h; the vacuum degree of the reactor is then increased to -0.08 to -0.095 MPa for 3h, and the thiol value is obtained by sampling and testing to obtain 74.6mgKOH / g, and the polycarbonate polyol with a number average molecular weight of 1500 can be obtained by unloading.
[0032] The difference between Preparation Example 9 and Preparation Example 4 is: Preparation of polycarbonate polyol with a number average molecular weight of 3000: 121g of 1,6-hexanediol, 277g of diethyl carbonate, 77.2g of ethylene glycol, 1.5g of tetrabutyl titanate, and 1g of antioxidant 1076 are put into a reactor, the temperature of the reactor is raised to 140°C, the outlet temperature at the top of the cooling tube is controlled at 126°C, the reactor temperature is gradually raised to 200°C at a heating rate of 15°C / h, and the reaction is kept at 200°C for 4h; the vacuum degree is maintained at -0.05 to -0.08 MPa for 3h; the vacuum degree of the reactor is then increased to -0.08 to -0.095 MPa for 3h, and the sampling test obtains a thiol value of 37.3mgKOH / g, and the polycarbonate polyol with a number average molecular weight of 3000 can be obtained by unloading.
[0033] The difference between Preparation Example 10 and Preparation Example 5 is: Preparation of polycarbonate polyol with a number average molecular weight of 1000: 194.5g of neopentyl glycol, 166g of dimethyl carbonate, 31.9g of ethylene glycol, 0.02g of tetra-tert-butyl titanate, and 0.03g of antioxidant 1076 are put into a reactor, the temperature of the reactor is raised to 140°C, the outlet temperature at the top of the cooling tube is controlled at 65°C, the temperature of the reactor is gradually raised to 200°C at a heating rate of 15°C / h, and the reaction is kept at 200°C for 2h; the vacuum degree is maintained at -0.05 to -0.08MPa for 2h; the vacuum degree of the reactor is then increased to -0.08 to -0.095 MPa for 2h, and the thiol value is obtained by sampling and testing to obtain 112mgKOH / g, and the polycarbonate polyol with a number average molecular weight of 1000 can be obtained by unloading. Example
[0034] A soft, highly wear-resistant and fold-resistant aliphatic polyurethane resin is prepared from aliphatic diisocyanate, polyol, chain extender, solvent, catalyst, terminator and functional additive. The total molar amount of active groups in polyol and chain extender is 0.95-1.10 times the molar amount of isocyanate group in aliphatic diisocyanate. The total molar amount of active groups in polyol and the molar amount of hydroxyl group in chain extender are prepared to be 1:(1.05-2.00).
[0035] The polyol is a polycarbonate thiol polyol with a number average molecular weight of 1000-3000 and at least one of a polyether polyol and a polyester polyol with a number average molecular weight of 1000-4000.
[0036] The polycarbonate thiol polyol comprises dithiol, diethyl carbonate, a catalyst and an antioxidant.
[0037] At least one of dithiol ethanedithiol, 1,3-propanedithiol, 1,4-butanedithiol, and 1,6-hexanedithiol.
[0038] The catalyst is at least one of tetrabutyl titanate, tetra-tert-butyl titanate and dibutyltin dilaurate.
[0039] The preparation method of polycarbonate thiol polyol is as follows: put dithiol, diethyl carbonate, a catalyst and an antioxidant into a reactor, raise the temperature of the reactor to 140-145°C, control the outlet temperature at the top of the cooling tube at 65-126°C, gradually raise the temperature of the reactor to 200-205°C at a heating rate of 15-20°C / h, and keep the temperature at 200°C for 2-4h; keep the vacuum degree at -0.05 to -0.08 MPa for 2-3h; then increase the vacuum degree of the reactor to -0.08 to -0.095 MPa for 2-3h, and take samples for testing to obtain polycarbonate thiol polyol with a hydroxyl value of 37.3-112mgKOH / g.
[0040] The aliphatic diisocyanate is at least one of isophorone diisocyanate, 4,4'-dicyclohexylmethane diisocyanate and hexamethylene diisocyanate.
[0041] The chain extender is at least one of diol and triol with a molecular weight of 61-500 g / mol.
[0042] The solvent is one or a mixture of two or more of dimethylformamide, methyl ethyl ketone, toluene, ethyl acetate, dimethyl carbonate and acetone.
[0043] The catalyst is organotin and / or organobismuth.
[0044] The terminator is at least one of methanol and ethanol.
[0045] The functional additives include at least one of an antioxidant, an ultraviolet absorber, a stabilizer, an anti-hydrolysis agent, and a flame retardant.
[0046] A method for preparing a soft, highly wear-resistant and folding-resistant aliphatic polyurethane resin comprises the following steps: Step 1, preparation of polycarbonate thiol polyol: put dithiol, diethyl carbonate, catalyst, and antioxidant into a reactor, raise the temperature of the reactor to 140-145°C, control the outlet temperature of the top of the cooling tube at 65-126°C, gradually raise the temperature of the reactor to 200-205°C at a heating rate of 15-20°C / h, and keep the temperature at 200°C for 2-4h; keep the vacuum degree at -0.05 to -0.08 MPa for 2-3h; then increase the vacuum degree of the reactor to -0.08 to -0.095 MPa for 2-3h, and take samples for testing to obtain polycarbonate thiol polyol with a hydroxyl value of 37.3-112mgKOH / g; Step 2: Add polyol, chain extender, solvent accounting for 20-30wt% of the total solvent mass, and functional additive into the reactor, heat to 45-50°C, and stir evenly; add aliphatic diisocyanate, control the kettle temperature at 85-90°C to react for 1-1.5h, add solvent accounting for 20-30wt% of the total solvent mass, control the reaction temperature at 88-92°C to continue the reaction, add the remaining solvent into the reactor as the viscosity increases, and add the catalyst until the viscosity reaches 4×10 3 -2×10 5 mPa•s / 25℃, add terminator to react for 30-90min, and unload to obtain soft, highly wear-resistant and folding-resistant aliphatic polyurethane resin.
[0047] Example 1: A soft, highly wear-resistant and fold-resistant aliphatic polyurethane resin is prepared from 100 g of 4,4′-dicyclohexylmethane diisocyanate, 100 g of the polycarbonate thiol polyol with a number average molecular weight of 2000 in Preparation Example 1, 100 g of polytetrahydrofuran diol with a number average molecular weight of 2000 (Hyosung Chemical), 13.3 g of ethylene glycol, 190 g of dimethyl carbonate, 500 g of dimethylformamide, 0.02 g of stannous octoate, 0.5 g of methanol, and 1 g of triphenyl phosphite. A method for preparing a soft, highly wear-resistant and folding-resistant aliphatic polyurethane resin comprises the following steps: Step 1, preparation of polycarbonate thiol polyol: see Preparation Example 1.
[0048] Step 2: Add 100g of polycarbonate thiol polyol with a number average molecular weight of 2000, 100g of polytetrahydrofuran diol with a number average molecular weight of 2000, 13.3g of ethylene glycol, 0.1g of antioxidant, and 500g of DMF in the reactor, stir evenly, add 100g of 4,4′-dicyclohexylmethane diisocyanate, control the kettle temperature at 85°C to react for 1h, add 0.02g of stannous octoate and continue to react for 2h, and add 190g of dimethyl carbonate DMC to the reactor as the viscosity increases; when the viscosity reaches 1.0×105 mPa·s / 25°C, add 0.5g of methanol to maintain the temperature at 85°C for 60min, unload, and obtain the final product - a soft, highly wear-resistant and fold-resistant aliphatic polyurethane resin.
[0049] The difference between Example 2 and Example 1 is that a soft, highly wear-resistant and folding-resistant aliphatic polyurethane resin is made from 79 g of isophorone diisocyanate IPDI, 200 g of polycarbonate thiol polyol with a number average molecular weight of 1500, 20 g of 1,4-butanediol, 699 g of dimethylformamide DMF, 0.01 g of bismuth carboxylate, 0.6 g of methanol, and 1 g of triphenyl phosphite.
[0050] A method for preparing a soft, highly wear-resistant and folding-resistant aliphatic polyurethane resin comprises the following steps: Step 1, preparation of polycarbonate thiol polyol: see Preparation Example 2; Step 2: Add 200 g of polycarbonate thiol polyol with a number average molecular weight of 1500 in Preparation Example 2, 1 g of triphenyl phosphite, 20 g of 1,4-butanediol, and 400 g of DMF into the reactor and stir evenly; add 79 g of IPDI, control the kettle temperature at 90 ° C to react for 2 h, add 200 g of DMF, control the reaction temperature at 90 ° C to continue the reaction, add 0.01 g of bismuth carboxylate, and add the remaining 99 g of DMF into the reactor as the viscosity increases until the viscosity reaches 0.6×10 5mPa·s / 25℃; add 0.6g of terminator methanol and react for 60min, then discharge to obtain the final product.
[0051] The difference between Example 3 and Example 1 is that a soft, highly wear-resistant and folding-resistant aliphatic polyurethane resin is made from 53g of hexamethylene diisocyanate HDI, 150g of the polycarbonate thiol polyol with a number average molecular weight of 1500 in Preparation Example 3, 120g of poly(1,6-hexanediol adipate) ester diol with a number average molecular weight of 3500, 25g of 1,6-hexanediol, 244g of methyl ethyl ketone, 800g of dimethylformamide DMF, 0.05g of dibutyltin dilaurate, 2g of ethanol, and 1g of antioxidant 1024.
[0052] A method for preparing a soft, highly wear-resistant and folding-resistant aliphatic polyurethane resin comprises the following steps: Step 1, preparation of polycarbonate thiol polyol: see Preparation Example 3; Step 2: 150 g of polycarbonate thiol polyol with a number average molecular weight of 1500, 1 g of antioxidant 1024, 25 g of 1,6-hexanediol, and 400 g of DMF in the reactor were added and stirred evenly; 53 g of HDI was added, the kettle temperature was controlled at 90 ° C for 2 h, 400 g of DMF was added, the reaction temperature was controlled at 90 ° C and the reaction was continued, 0.05 g of dibutyltin dilaurate was added, and 244 g of MEK was added to the reactor as the viscosity increased until the viscosity reached 2×10 4 mPa·s / 25℃; add 2g of ethanol as terminator and react for 80min, then discharge to obtain the final product.
[0053] The difference between Example 4 and Example 1 is that a soft, highly wear-resistant and folding-resistant aliphatic polyurethane resin is prepared by 156 g of 4,4′-dicyclohexylmethane diisocyanate, 200 g of the polycarbonate thiol polyol with a number average molecular weight of 3000 in Preparation Example 4, 100 g of polypropylene oxide diol with a number average molecular weight of 2000 (Shanghai Dongda Chemical Co., Ltd.), 100 g of polytetrahydrofuran diol with a number average molecular weight of 3000 (Xiaoxing Chemical), 100 g of polyethylene adipate glycol 1,4-butylene glycol ester diol with a number average molecular weight of 2000 (Zhejiang Hexin Technology Co., Ltd.), 30 g of 1,3-propylene glycol, 10,000 g of dimethylformamide, 600 g of toluene, 0.03 g of dibutyltin dilaurate, 2 g of methanol, and 2 g of triphenyl phosphite.
[0054] A method for preparing a soft, highly wear-resistant and folding-resistant aliphatic polyurethane resin comprises the following steps: Step 1, preparation of polycarbonate thiol polyol: see Preparation Example 4; Step 2: Add 200g of the polycarbonate thiol polyol with a number average molecular weight of 3000 in Preparation Example 4, 100g of polypropylene oxide diol with a number average molecular weight of 2000, 100g of polytetrahydrofuran diol with a number average molecular weight of 3000, 100g of polyethylene adipate glycol 1,4-butylene glycol ester diol with a number average molecular weight of 2000, 1g of triphenyl phosphite, and 1000g of DMF into the reactor, heat to 45°C, and stir evenly; add 156g of 4,4′-dicyclohexylmethane diisocyanate, control the kettle temperature at 90°C to react for 1h, add 300g of toluene, control the reaction temperature at 90°C to continue the reaction, add 9000g of dimethylformamide and 300g of toluene into the reactor as the viscosity increases, add a catalyst until the viscosity reaches 6.5×10 4 mPa·s / 25℃; add 2g of methanol as terminator and react for 60min, then discharge to obtain the final product.
[0055] The difference between Example 5 and Example 1 is that a soft, highly wear-resistant and folding-resistant aliphatic polyurethane resin is prepared from 128g of isophorone diisocyanate, 200g of the polycarbonate thiol polyol with a number average molecular weight of 1000 in Preparation Example 5, 125g of polyethylene adipate glycol 1,2-propylene glycol ester diol with a number average molecular weight of 1500 (source: Zhejiang Hexin Technology Co., Ltd.), 18g of ethylene glycol, 300g of dimethylformamide DMF, 800g of methyl ethyl ketone, 0.03g of dibutyl tin dilaurate, 1g of methanol, and 1g of antioxidant 1010.
[0056] A method for preparing a soft, highly wear-resistant and folding-resistant aliphatic polyurethane resin comprises the following steps: Step 1, preparation of polycarbonate thiol polyol: see Preparation Example 5; Step 2: Add 200 g of the polycarbonate thiol polyol with a number average molecular weight of 1000 in Preparation Example 5, 125 g of polyethylene adipate glycol 1,2-propylene glycol ester diol with a number average molecular weight of 1500, 1 g of antioxidant 1010, and 300 g of DMF into the reactor, heat to 45 ° C, and stir evenly; add 128 g of isophorone diisocyanate, control the kettle temperature at 90 ° C to react for 1 hour, add 500 g of methyl ethyl ketone, control the reaction temperature at 90 ° C to continue the reaction, add the remaining 300 g of methyl ethyl ketone into the reactor as the viscosity increases, and add the catalyst until the viscosity reaches 4.5×10 4 mPa·s / 25℃; add 1 g of methanol as terminator and react for 60 min, then discharge to obtain the final product.
[0057] The difference between Example 6 and Example 3 is that a soft, highly wear-resistant and folding-resistant aliphatic polyurethane resin is made of 53g of hexamethylene diisocyanate HDI, 150g of the polycarbonate thiol polyol with a number average molecular weight of 1500 in Preparation Example 3, 120g of poly(1,6-hexanediol adipate) ester diol with a number average molecular weight of 3500, 25g of 1,6-hexanediol, 244g of methyl ethyl ketone, 1000g of dimethylformamide DMF, 0.05g of dibutyltin dilaurate, 2g of ethanol, 1g of antioxidant 1024, and 5g of surface-amino-modified nano-aramid fiber.
[0058] Preparation method of surface amino-modified nano-aramid fiber: Step 1: Cut DuPont Kevlar-49 fiber into 0.5 mm pieces, extract with acetone and distilled water for 12 h, and heat at 60 ℃ vacuum oven for 24h to obtain Kevlar chopped fibers with a length of 0.5mm, and vacuum dried at 120℃ for 2h; at the same time, weigh 2.16g methanol, 2.5g potassium tert-butoxide and 1.0L dimethyl sulfoxide DMSO, magnetically stir at 50℃ for 4h to obtain a transparent liquid DMSO solution, and cool to room temperature; take 2g of Kevlar chopped fibers with a length of 0.5mm that have completed vacuum drying and add them to the DMSO solution configured above, after nitrogen replaces oxygen, add 20g of 8wt.% potassium hydroxide aqueous solution to the DMSO solution at a dropping speed of 1mL / min, magnetically stir at 500rpm for 12h at room temperature, add 1.0L distilled water drop by drop, and continue to magnetically stir at 500rpm for 12h, vacuum filter and use distilled water to adjust the pH to neutral, wash the obtained precipitate with acetone and vacuum dry it in turn, and you can get nano aramid fiber ANF; Step 2: treating the obtained nano-aramid fiber ANF with low-temperature plasma, wherein the low-temperature plasma treatment gas is air, the treatment temperature is 4° C., and the low-temperature plasma treatment time is 100 s, so that active hydroxyl groups are formed on the surface of the nano-aramid fiber ANF; Step three, the nano-aramid fiber ANF obtained in step two is dispersed in distilled water to obtain a 0.5wt% ANF dispersion, 100mL of the 0.5wt% ANF dispersion is weighed, 2g of KH550-γ-aminopropyltriethoxysilane is added, and the mixture is magnetically stirred at 400rpm for 5min, and ultrasonic dispersion treatment is performed with an ultrasonic frequency of 44kHz and an ultrasonic power of 600W. After ultrasonic treatment for 30min, vacuum filtration and vacuum drying are performed in sequence to obtain the surface amino-modified nano-aramid fiber.
[0059] A method for preparing a soft, highly wear-resistant and folding-resistant aliphatic polyurethane resin comprises the following steps: Step 1, preparation of polycarbonate thiol polyol: see Preparation Example 3; Step 2: 150 g of polycarbonate thiol polyol with a number average molecular weight of 1500, 1 g of antioxidant 1024, 25 g of 1,6-hexanediol, 5 g of surface amino-modified nano-aramid fiber, and 600 g of DMF are added to the reactor and stirred evenly; 53 g of HDI is added, the kettle temperature is controlled at 90 ° C for reaction for 2 h, 400 g of DMF is added, the reaction temperature is controlled at 90 ° C to continue the reaction, 0.05 g of dibutyltin dilaurate is added, and 244 g of MEK is added to the reactor as the viscosity increases until the viscosity reaches 2×10 4 mPa·s / 25℃; add 2g of ethanol as terminator and react for 80min, then discharge to obtain the final product.
[0060] The difference between Comparative Example 1 and Example 1 is that the polycarbonate thiol polyol with a number average molecular weight of 2000 in Preparation Example 1 is replaced by the polycarbonate polyol with a number average molecular weight of 2000 in Preparation Example 6.
[0061] The difference between Comparative Example 2 and Example 1 is that the polycarbonate thiol polyol with a number average molecular weight of 1500 in Preparation Example 2 is replaced by the polycarbonate polyol with a number average molecular weight of 1500 in Preparation Example 7.
[0062] The difference between Comparative Example 3 and Example 1 is that the polycarbonate thiol polyol with a number average molecular weight of 1500 in Preparation Example 3 is replaced by the polycarbonate polyol with a number average molecular weight of 1500 in Preparation Example 8.
[0063] The difference between Comparative Example 4 and Example 1 is that the polycarbonate thiol polyol with a number average molecular weight of 3000 in Preparation Example 4 is replaced by the polycarbonate polyol with a number average molecular weight of 3000 in Preparation Example 9.
[0064] The difference between Comparative Example 5 and Example 1 is that the polycarbonate thiol polyol with a number average molecular weight of 1000 in Preparation Example 5 is replaced by the polycarbonate polyol with a number average molecular weight of 1000 in Preparation Example 10.
[0065] Performance test: Preparation of samples: Scrape 0.15 mm of the polyurethane resin in Examples 1-5 and Comparative Examples 1-5 on release paper, dry and shape in an oven at 120°C, repeat the scraping once to a thickness of 0.15 mm, and then dry and shape in an oven at 120°C to obtain a resin film, and then use an adhesive to stick the resin film on the release paper to the microfiber base of Hexin Kuraray to obtain a test synthetic leather sample.
[0066] 1. Wear resistance is tested according to GMW 3208-2012 rotational wear test.
[0067] 2. The folding resistance is measured according to the QB / T 4197-2011 test method, and the number of bends is tested at -20℃.
[0068] Table 1: Test parameters of synthetic leather in Examples 1-6 and Comparative Examples 1-5
[0069] Combining Examples 1-5 and Comparative Examples 1-5 and Table 1, it can be seen that the soft, highly wear-resistant and highly folding-resistant aliphatic polyurethane resin prepared using polycarbonate thiol polyol has similar wear resistance properties as polycarbonate polyol under the same formula. However, the cold resistance and folding resistance of the synthetic leather prepared using the soft, highly wear-resistant and highly folding-resistant aliphatic polyurethane resin in the present application are greatly improved, and significant technological progress has been achieved.
[0070] Combining Example 3 and Example 6 with Table 1, it can be seen that the addition of surface amino-modified nano-aramid fiber can improve the wear resistance of synthetic leather prepared from soft, highly wear-resistant and highly folding-resistant aliphatic polyurethane resin, and also has a positive effect on the cold resistance and folding resistance of synthetic leather prepared from soft, highly wear-resistant and highly folding-resistant aliphatic polyurethane resin. Adding surface amino-modified nano-aramid fiber to the formula of soft, highly wear-resistant and highly folding-resistant aliphatic polyurethane resin with low hardness and relatively soft texture can improve the wear resistance and cold resistance and folding resistance of synthetic leather prepared therefrom.
[0071] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A soft, highly wear-resistant and folding-resistant aliphatic polyurethane resin, characterized in that: It is made of aliphatic diisocyanate, polyol, chain extender, solvent, catalyst, terminator and functional additive; The polyol is a polycarbonate thiol polyol with a number average molecular weight of 1000-3000 and at least one of a polyether polyol and a polyester polyol with a number average molecular weight of 1000-4000; The polycarbonate thiol polyol is made of dithiol, diethyl carbonate, a catalyst and an antioxidant; At least one of the dithiol ethanedithiol, 1,3 propanedithiol, 1,4 butanedithiol, and 1,6 hexanedithiol; The catalyst is at least one of tetrabutyl titanate, tetra-tert-butyl titanate, and dibutyltin dilaurate; The aliphatic diisocyanate is at least one of isophorone diisocyanate, 4,4′-dicyclohexylmethane diisocyanate and hexamethylene diisocyanate; The chain extender is at least one of a diol or a triol having a molecular weight of 61-500 g / mol; The solvent is one or a mixture of two or more of dimethylformamide, methyl ethyl ketone, toluene, ethyl acetate, dimethyl carbonate, and acetone; The catalyst is organic tin and / or organic bismuth; The terminator is at least one of methanol and ethanol; The functional additives include at least one of an antioxidant, an ultraviolet absorber, a stabilizer, an anti-hydrolysis agent, and a flame retardant.
2. The soft, highly wear-resistant and folding-resistant aliphatic polyurethane resin according to claim 1, characterized in that: The preparation method of the polycarbonate thiol polyol is as follows: dithiol, diethyl carbonate, a catalyst and an antioxidant are added into a reaction kettle, the temperature of the reaction kettle is raised to 140-145°C, the outlet temperature at the top of the cooling tube is controlled at 65-126°C, the temperature of the kettle is gradually raised to 200-205°C at a heating rate of 15-20°C / h, and the reaction is kept at 200°C for 2-4h; the vacuum degree is maintained at -0.05 to -0.08MPa for 2-3h; the vacuum degree of the reaction kettle is then increased to -0.08 to -0.095MPa for 2-3h, and a polycarbonate thiol polyol with a hydroxyl value of 37.3-112mgKOH / g is obtained by sampling and testing.
3. The soft, highly wear-resistant and folding-resistant aliphatic polyurethane resin according to claim 1, characterized in that: The total molar amount of active groups in the polyol and the chain extender is 0.95-1.10 times the molar amount of isocyanate groups in the aliphatic diisocyanate.
4. The soft, highly wear-resistant and folding-resistant aliphatic polyurethane resin according to claim 3, characterized in that: The total molar amount of active groups in the polyol and the molar amount of hydroxyl groups in the chain extender are prepared as 1:(1.05-2.00).
5. The soft, highly wear-resistant and folding-resistant aliphatic polyurethane resin according to claim 4, characterized in that: The invention is prepared from 4,4'-dicyclohexylmethane diisocyanate, polycarbonate thiol polyol with a number average molecular weight of 2000, polytetrahydrofuran diol with a number average molecular weight of 2000, ethylene glycol, dimethyl carbonate, dimethylformamide, stannous octoate, methanol and triphenyl phosphite.
6. The soft, highly wear-resistant and folding-resistant aliphatic polyurethane resin according to claim 4, characterized in that: The invention is prepared from isophorone diisocyanate, polycarbonate thiol polyol with a number average molecular weight of 1500, 1,4-butanediol, dimethylformamide, bismuth carboxylate, methanol and triphenyl phosphite.
7. The soft, highly wear-resistant and folding-resistant aliphatic polyurethane resin according to claim 4, characterized in that: The invention is prepared from hexamethylene diisocyanate, polycarbonate thiol polyol with a number average molecular weight of 1500, poly 1,6-hexanediol adipate diol with a number average molecular weight of 3500, 1,6-hexanediol, methyl ethyl ketone, dimethylformamide, dibutyltin dilaurate, ethanol and antioxidant 1024.
8. The soft, highly wear-resistant and folding-resistant aliphatic polyurethane resin according to claim 4, characterized in that: The invention is prepared from 4,4'-dicyclohexylmethane diisocyanate, polycarbonate thiol polyol with a number average molecular weight of 3000, polypropylene oxide diol with a number average molecular weight of 2000, polytetramethylene oxide diol with a number average molecular weight of 3000, polyethylene adipate glycol 1,4-butylene glycol ester diol with a number average molecular weight of 2000, 1,3-propylene glycol, dimethylformamide, toluene, dibutyltin dilaurate, methanol and triphenyl phosphite.
9. The soft, highly wear-resistant and folding-resistant aliphatic polyurethane resin according to claim 4, characterized in that: The invention is prepared from isophorone diisocyanate, polycarbonate thiol polyol with a number average molecular weight of 1000, polyethylene adipate 1,2-propylene glycol ester diol with a number average molecular weight of 1500, ethylene glycol, dimethylformamide, methyl ethyl ketone, dibutyl tin dilaurate, methanol and antioxidant 1010.
10. A method for preparing the soft, highly wear-resistant and folding-resistant aliphatic polyurethane resin according to any one of claims 1 to 9, characterized in that: The following steps are involved: Step 1, preparation of polycarbonate thiol polyol; Step 2: Add polyol, chain extender, solvent accounting for 20-30wt% of the total solvent mass, and functional additive into the reactor, heat to 45-50°C, and stir evenly; add aliphatic diisocyanate, control the kettle temperature at 85-90°C to react for 1-1.5h, add solvent accounting for 20-30wt% of the total solvent mass, control the reaction temperature at 88-92°C to continue the reaction, add the remaining solvent into the reactor as the viscosity increases, and add the catalyst until the viscosity reaches 4×10 3 -2×10 5 mPa•s / 25℃, add terminator to react for 30-90min, and unload to obtain soft, highly wear-resistant and folding-resistant aliphatic polyurethane resin.