Benzotriazole modified anti-sagging resin as well as preparation method and coating thereof
By reacting benzotriazole-type aging resistance additive with polyurea compounds in the sag-resistant resin to generate polyurea crystals, the problems of single properties and poor stability of traditional resins are solved, and high aging resistance and sag-resistant resistance are achieved , while avoiding environmental and health pollution and simplifying production processes.
Patent Information
- Application Number
- CN202411212315.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-11-08
AI Technical Summary
Traditional anti-sag resins have single properties and poor long-term stability. The addition of aging-resistant agents may lead to incompatibility, pollution of the environment and harming health.
A benzotriazole-based aging-resistant additive is used as the raw material of the polyurea compound for the anti-sag resin. The polyurea crystal is generated by reacting with diisocyanate to avoid volatile and compatibility issues and enhance the aging resistance of the resin.
The resin has high aging resistance and sag resistance, avoids the stratification and volatility of traditional additives, simplifies the production process, and improves product quality and stability.
Smart Images

Figure CN118909221A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of coating additives, and in particular relates to a benzotriazole-modified anti-sagging resin and a preparation method thereof, and a coating. Background Art
[0002] Resin materials are widely used in coatings, composite materials, electronic packaging and construction. These applications have high requirements for the aging resistance of resins to ensure the long-term stability and service life of products. However, resins will be affected by environmental factors (such as ultraviolet rays, temperature, humidity, etc.) during long-term use, resulting in gradual performance decline, embrittlement, color change and reduced mechanical properties.
[0003] In order to improve the aging properties of the resin, anti-aging agents, modifiers or other functional additives are usually added to it. However, these additives may be at risk of being incompatible with the coating resin matrix, which may lead to unstable performance, such as stratification or precipitation. In addition, the introduction of additives may also affect the processing properties of the resin, such as fluidity and curing speed, thereby affecting production efficiency and product quality. Since many anti-aging agents and modifiers are small molecule compounds and are volatile, they may have potential negative effects on the environment or human health during use and need to be carefully considered. In addition, the addition of new additives or modifiers may require adjustments to the production process of the coating, increasing the complexity of the process and the difficulty of management. Therefore, the research and introduction of new functional materials to replace traditional anti-aging agents and modifiers has become an urgent problem to be solved.
[0004] Paints with anti-sagging properties are a type of paint that has anti-sagging additives added to change its rheological properties. The main function of this type of paint is to prevent the paint from flowing when painting on vertical or inclined surfaces, resulting in uneven coating thickness or accumulation. The main principle of anti-sagging additives is to modify the resin matrix in the paint through polyurea compounds. The molecular structure of polyurea compounds easily forms hydrogen bonds, which makes the paint show higher viscosity when it is not subjected to or subjected to small external forces (such as slight gravity on a vertical surface), thereby reducing sagging. When a certain shear force is applied (such as during transportation or spraying), the hydrogen bonds are destroyed, and the resin shows lower viscosity and is easy to flow. Anti-sagging resins are mainly used for spraying large vertical surfaces or other applications that require anti-sagging. However, the anti-sagging resins currently on the market have a single performance. Although the initial performance has improved, aging, discoloration or performance degradation may occur during long-term use, affecting their long-term stability.
[0005] In summary, traditional anti-sagging resins have problems such as single performance and poor long-term stability. Directly adding anti-aging agents to coatings to improve their aging resistance will bring negative effects such as incompatibility, affect anti-sagging performance, pollute the environment and harm health. Summary of the invention
[0006] In view of the above technical problems, the present invention takes a new approach, using a benzotriazole anti-aging agent as a synthetic raw material for an anti-sagging resin, i.e., a polyurea compound, so that the benzotriazole anti-aging agent exists in the form of polyurea crystals, thereby avoiding its volatilization risk and incompatibility with the coating, and also enhancing the aging resistance of the anti-sagging resin. Therefore, the present invention provides a benzotriazole-modified anti-sagging resin, a preparation method thereof, and a coating.
[0007] To achieve the above object, the technical solution of the present invention is:
[0008] A benzotriazole modified anti-sagging resin, calculated by weight, comprises the following components:
[0009]
[0010] Preferably, the chemical structure of the primary amino-containing benzotriazole is:
[0011]
[0012] Where R 1 —R 8 It is any one of the structures -H, -OH, -OCH3, -C4H9, -Cl and -OCH2CHOCH2, or any combination thereof; n=0-10.
[0013] Preferably, the chemical structure of the primary amino-containing benzotriazole is:
[0014] That is, R1-R8 are all -H; or
[0015] That is, R8 = -NH2, and R1-R7 are all -H.
[0016] Preferably, the solvent is any one or more of xylene, S-100A high boiling point solvent or S-150 aromatic solvent.
[0017] Preferably, when the solvent is a mixed solvent of any two of xylene, S-100A high boiling point solvent or S-150 aromatic solvent, the arbitrary blending ratio is 1:0-10.
[0018] Preferably, the polymer resin is polyacrylic resin (PA) or / and polyester resin (PE).
[0019] Preferably, the isocyanate is any one of hexamethylene diisocyanate (HDI), diphenylmethane-4,4'-diisocyanate (MDI) or 4,4'-dicyclohexylmethane diisocyanate (HMDI) or a mixture thereof.
[0020] Based on the same inventive concept, the present invention also provides a method for preparing the benzotriazole-modified anti-sagging resin, comprising the following steps:
[0021] S1: mixing primary aminobenzhydrol with part of the solvent to prepare a primary aminobenzhydrol solution of a preset concentration;
[0022] S2: The polymer resin and the remaining solvent are mixed uniformly in a reaction kettle and stirred continuously, the temperature of the reaction system is maintained at 0-40° C., the primary aminobenzhydrol solution prepared in step S1 is dispersed into the reaction system, and diisocyanate is added and stirred to obtain the modified anti-sagging resin.
[0023] Based on the same inventive concept, the present invention also provides a coating, comprising the benzotriazole-modified anti-sagging resin.
[0024] Due to the adoption of the above technical solution, the present invention has the following advantages and positive effects compared with the prior art:
[0025] The modified anti-sagging resin provided by the present invention comprises a polymer resin, a solvent, a plurality of or a mixed diisocyanate, and a primary amino-containing benzotriazole. The primary amino-containing benzotriazole is used as a polyurea raw material, and a primary amine and primary amino group in the molecular structure react with the diisocyanate to form a polyurea crystal, thereby achieving the anti-sagging function of the resin, so that the benzotriazole ultraviolet light absorber exists in the form of a polyurea crystal, and the benzotriazole ultraviolet light absorber becomes a part of the polyurea structure, thereby avoiding the volatility problem of the small molecule compound of the benzotriazole ultraviolet light absorber, thereby avoiding the problem of environmental pollution and health hazards, and is more environmentally friendly and safer than the prior art.
[0026] In addition, the benzotriazole ultraviolet light absorber exists in the form of polyurea crystals, and together with the polymer resin, it constitutes polyurea resin. When added to the coating, due to the principle of similar compatibility, it is evenly dispersed with the coating, thus avoiding the problems of stratification and precipitation between the anti-aging agent and the coating.
[0027] At the same time, the present invention introduces benzotriazole into the polyurea resin in the form of a chemical bond, so that benzotriazole becomes a group in the molecular structure of the polyurea, which not only does not affect the anti-sagging performance of the resin, but also significantly enhances the aging resistance of the resin, prolongs its service life, and makes the anti-sagging resin have both anti-sagging and aging resistance. It is added to the coating in the form of an additive, which brings the same function to the coating while avoiding the stratification and volatility problems of traditional anti-aging additives, and simplifies the coating production process. Compared with the prior art, it reduces the complexity of the coating process and improves production efficiency and product quality.
[0028] The modified anti-sagging resin preparation method provided by the present invention is to add and disperse a solution containing primary aminobenzotriazole into a reaction system consisting of a polymer resin and a solvent, and then add diisocyanate to the reaction system for stirring and reacting, thereby improving the synthesis process of the resin and enhancing the consistency and stability of the product. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 The rheological properties test results of the resin of Example 1 of the present invention;
[0030] Figure 2 The rheological properties test results of the resin of Example 2 of the present invention;
[0031] Figure 3 The rheological properties test results of the resin of Example 3 of the present invention;
[0032] Figure 4 The rheological properties test results of the resin of Comparative Example 1 of the present invention are as follows;
[0033] Figure 5 The rheological properties test results of the resin of Comparative Example 2 of the present invention are as follows;
[0034] Figure 6 The following are the rheological properties test results of the resin of Comparative Example 3 of the present invention. DETAILED DESCRIPTION
[0035] Benzotriazole anti-aging additives have become an important choice for improving the weather resistance of resin materials due to their excellent UV absorption performance. This type of additive effectively prevents the damage of photooxidation reactions to resins by absorbing UV rays and converting them into harmless heat energy, thereby delaying the aging of materials. Since benzotriazole compounds can effectively absorb UV rays in the UV-A and UV-B bands, they are widely used in coatings, composite materials, electronic packaging and building materials to significantly improve the durability and service life of products.
[0036] The present invention selects benzotriazole anti-aging additives. Since polyurea is an amino group and an isocyanate for polymerization reaction, a primary amino-containing benzotriazole is selected to react with an isocyanate to synthesize polyurea, and benzotriazole becomes a group of the polyurea molecular structure. Moreover, since the molecular structure of benzotriazole is highly symmetrical and contains a rigid aromatic ring, it is helpful to form a regular segment arrangement, thereby improving the crystallinity of the polyurea. Furthermore, the molecular group of benzotriazole will not affect the polyurea crystal, but will also improve the crystallinity of the polyurea. Furthermore, the present invention selects a primary amino-containing benzotriazole to introduce an anti-aging agent into the anti-sagging resin matrix in a chemically combined manner, and under the premise of not affecting the anti-sagging performance, the volatility and compatibility of the anti-aging agent are overcome, and the anti-aging performance of the anti-sagging resin is improved.
[0037] It should be noted that: the benzotriazole anti-aging additives in the current market generally adopt an external addition method, which leads to insufficient compatibility between the additive and the resin matrix, which may cause phenomena such as stratification and precipitation, and affect the performance and quality of the coating. In addition, the traditional addition method often needs to adjust the production process, thereby increasing the process complexity and management difficulty. The present invention directly introduces the benzotriazole additive into the synthesis process of the anti-sagging resin by using primary amino-containing benzotriazole as a raw material, ensuring the high compatibility of the additive with the resin matrix, simplifying the production process, and improving the consistency and stability of the product.
[0038] The benzotriazole additives currently used are usually volatile organic compounds (VOCs), which release harmful substances during use, not only polluting the environment, but also causing potential harm to human health. In addition, the presence of volatile substances will also affect the long-term stability of the resin, leading to performance degradation. The present invention introduces the benzotriazole ultraviolet light absorber into the polyurea resin in the form of a chemical bond, so that benzotriazole becomes a group of the polyurea molecular structure, effectively reducing the volatility problem, providing a more environmentally friendly and safe solution, and significantly improving the durability and aging resistance of the resin.
[0039] Existing anti-sagging resins can effectively reduce sagging in the initial stage of use, but are prone to aging, discoloration and performance degradation during long-term use, thereby affecting the service life of coating products. The present invention introduces primary amino benzotriazole into the polyurea structure, which not only effectively improves the anti-sagging performance in the initial stage, but also significantly enhances the aging resistance and long-term stability of the resin, prolongs its long-term service life, and overcomes the shortcomings of the prior art.
[0040] The following is a further detailed description of a benzotriazole modified anti-sagging resin and its preparation method and coating proposed by the present invention in conjunction with the accompanying drawings and specific embodiments. The advantages and features of the present invention will become more clear according to the following description.
[0041] Example 1: Bz-A compound + HDI + HMDI in PA resin
[0042] In a 1000mL dispersion tank equipped with a high-speed dispersion disk and a thermometer, 447.50g PA (solid content: 70.00%) and 72.83g xylene were added in sequence, nitrogen was introduced, and the mixture was stirred evenly at 1000rpm. When the temperature in the tank was 23°C, 16.45g (77.55mmol) of the Bz-A compound + 15g of the xylene mixed solution was quickly added dropwise to the dispersion tank, and the mixture was stirred and dispersed at 4000rpm for 1 minute. Then 6.38g (37.93mmol) of HDI was added to the dispersion tank, the stirring rate was increased to 4000rpm, and the mixture was dispersed for 2 minutes. Then 4.97g (18.96mmol) of HMDI was added, and the mixture was dispersed at 4000rpm for 40 minutes to obtain an opaque thixotropic resin R1 with a fineness of ≤10μm. A portion of the R1 resin was sealed and placed in a 50°C water bath under 20W UVA-340 lamp for storage for 10 days, then taken out and marked as hot-stored resin R1', with a fineness of ≤10 μm.
[0043] The high shear (1000s) of resin R1 and R1' after 10 days of heat storage (50°C) and illumination (20W UVA-340) were measured by rotational rheometer. -1 ) and low shear viscosity (1s -1 ) changes and determine the shear factor.
[0044] Example 2 Bz-A compound + HDI + HMDI in PE resin
[0045] In a 1000mL dispersion tank equipped with a high-speed dispersion disk and a thermometer, 423.30g of PE (solid content: 72.00%) and 97.16g of xylene were added in sequence, nitrogen was introduced, and the mixture was stirred evenly at 1000rpm. When the temperature in the tank was 23°C, 16.45g (77.55mmol) of Bz-A compound + 15g of xylene mixed solution was quickly added dropwise to the dispersion tank, and the mixture was stirred and dispersed at 4000rpm for 1 minute. Then 6.38g (37.93mmol) of HDI was added to the dispersion tank, the stirring rate was increased to 4000rpm, and the mixture was dispersed for 2 minutes. Then 4.97g (18.96mmol) of HMDI was added, and the mixture was dispersed at 4000rpm for 40 minutes to obtain an opaque resin R2 with a fineness of ≤10μm. A portion of the R2 resin was sealed and placed in a 50°C water bath under 20W UVA-340 lamp for storage for 10 days, and was marked as the resin after hot storage R2', with a fineness of ≤10 μm.
[0046] The high shear (1000s) of resin R2 and R2' after 10 days of heat storage (50°C) and illumination (20W UVA-340) were measured by rotational rheometer. -1 ) and low shear viscosity (1s -1 ) changes and determine the shear factor.
[0047] Example 3 Bz-B compound + MDI + HMDI in PA
[0048] In a 1000mL dispersion tank equipped with a high-speed dispersion disk and a thermometer, 447.50g of PA (solid content: 70.00%) and 72.83g of xylene were added in sequence, nitrogen was introduced, and the mixture was stirred evenly at 1000rpm. When the temperature in the tank was 23°C, 17.60g (77.55mmol) of the Bz-B compound + 15g of the xylene mixed solution was quickly added dropwise to the dispersion tank, and the mixture was stirred and dispersed at 4000rpm for 1 minute. Then 9.49g (37.93mmol) of MDI was added to the dispersion tank, the stirring rate was increased to 4000rpm, and the mixture was dispersed for 2 minutes. Then 4.97g (18.96mmol) of HMDI was added, and the mixture was dispersed at 4000rpm for 40 minutes to obtain an opaque thixotropic resin R3 with a fineness of ≤10μm. A portion of the R3 resin was sealed and placed in a 50°C water bath under 20W UVA-340 lamp for 10 days, then taken out and marked as hot-stored resin R3', with a fineness of ≤10 μm.
[0049] The high shear (1000s) of resin R3 and R3' after 10 days of heat storage (50°C) and illumination (20W UVA-340) were measured by rotational rheometer. -1 ) and low shear viscosity (1s -1 ) changes and determine the shear factor.
[0050] Comparative Example 1: Benzylamine + HDI + HMDI in PA
[0051] In a 1000mL dispersion tank equipped with a high-speed dispersion disk and a thermometer, 447.50g of PA (solid content: 70.00%) and 87.83g of xylene were added in sequence, nitrogen was introduced, and the mixture was stirred evenly at 1000rpm. When the temperature in the tank was 23°C, 8.31g (77.55mmol) of benzylamine was quickly added dropwise to the dispersion tank, and the mixture was stirred and dispersed at 4000rpm for 1 minute. Then, 6.38 g (37.93 mmol) of HDI was added to the dispersion tank, and the stirring rate was increased to 4000 rpm. After dispersion for 2 minutes, 4.97 g (18.96 mmol) of HMDI was added, and dispersion was carried out at 4000 rpm for 40 minutes to obtain an opaque thixotropic resin R4 with a fineness of ≤10 μm. Part of the R4 resin was sealed and placed in a 50°C water bath under 20 W UVA-340 lamp for storage for 10 days, and then taken out and marked as resin R4' after hot storage. The fineness was measured to be ≤10 μm.
[0052] The high shear (1000s) of resin R4 and R4' after 10 days of heat storage (50°C) and illumination (20W UVA-340) was measured by rotational rheometer. -1) and low shear viscosity (1s -1 ) changes and determine the shear factor.
[0053] Comparative Example 2: Benzylamine + HDI + HMDI in PE
[0054] In a 1000mL dispersion tank equipped with a high-speed dispersion disk and a thermometer, 423.30g of PE (solid content: 72.00%) and 112.16g of xylene were added in sequence, nitrogen was introduced, and the mixture was stirred evenly at 1000rpm. When the temperature in the tank was 23°C, 8.31g (77.55mmol) of benzylamine was quickly added dropwise to the dispersion tank, and the mixture was stirred and dispersed at 4000rpm for 1 minute. Then, 6.38 g (37.93 mmol) of HDI was added to the dispersion tank, and the stirring rate was increased to 4000 rpm. After dispersion for 2 minutes, 4.97 g (18.96 mmol) of HMDI was added, and dispersion was carried out at 4000 rpm for 40 minutes to obtain an opaque resin R5 with a fineness of ≤10 μm. Part of the R5 resin was sealed and placed in a 50°C water bath under 20 W UVA-340 lamp for storage for 10 days, then taken out and marked as resin R5' after hot storage. The fineness was measured to be ≤10 μm.
[0055] The high shear (1000s) of resin R5 and R5' after 10 days of heat storage (50°C) and illumination (20W UVA-340) were measured by rotational rheometer. -1 ) and low shear viscosity (1s -1 ) changes and determine the shear factor.
[0056] Comparative Example 3: Benzylamine + MDI + HMDI in PA
[0057] In a 1000mL dispersion tank equipped with a high-speed dispersion disk and a thermometer, 447.50g of PA (solid content: 70.00%) and 87.83g of xylene were added in sequence, nitrogen was introduced, and the mixture was stirred evenly at 1000rpm. When the temperature in the tank was 23°C, 8.31g (77.55mmol) of benzylamine was quickly added dropwise to the dispersion tank, and the mixture was stirred and dispersed at 4000rpm for 1 minute. Then, 9.49 g (37.93 mmol) of MDI was added to the dispersion tank, and the stirring rate was increased to 4000 rpm. After dispersion for 2 minutes, 4.97 g (18.96 mmol) of HMDI was added, and dispersion was carried out at 4000 rpm for 40 minutes to obtain an opaque thixotropic resin R6 with a fineness of ≤10 μm. Part of the R6 resin was sealed and placed in a 50°C water bath under 20 W UVA-340 lamp for storage for 10 days, then taken out and marked as resin R6' after hot storage. The fineness was measured to be ≤10 μm.
[0058] The high shear (1000s) of resin R6 and R6' after 10 days of heat storage (50°C) and illumination (20W UVA-340) were measured by rotational rheometer. -1 ) and low shear viscosity (1s -1 ) changes and determine the shear factor.
[0059] The above-mentioned fineness test is measured in accordance with the national standard GB / T 1724-2019.
[0060] According to the conventional detection method in the art, the above resin is subjected to rheological behavior test
[0061] Test instrument model: Test conditions: 10# rotor, temperature: 25℃, speed is divided into two sections, the first section: 1000s -1 Cutting time: 5 minutes; second section: 1s -1 Cutting time 9 minutes.
[0062] Shear factor: Calculate according to the following formula: X = A0 / A1. Where A0 is the sample rotation speed of 1s -1 The viscosity at A1 is the sample speed of 1000s -1 The viscosity at .
[0063] The shear viscosity test results of the resins of Examples 1-3 and Comparative Examples 1-3 before and after heat storage are as follows: Figure 1-6 The rheological properties test results are shown in Table 1. Figure 1-3 It can be concluded that the obtained resin has anti-sagging performance before and after heat storage, indicating that the polyurea synthesized with primary aminobenzotriazole as raw material can also have anti-sagging performance. Figure 1-6 It can be seen from the comparison that the shear viscosity of the resins in Examples 1-3 is basically unchanged before and after heat storage, while the shear viscosity of the resins in Comparative Examples 1-3 is reduced after heat storage.
[0064] Table 1 Test results of viscosity and shear factor of resin before and after heat storage of Examples 1-3 and Comparative Examples 1-3
[0065]
[0066] By comparing the low shear viscosity and shear factor before and after heat storage, it can be seen that the viscosity of Examples 1-3 does not change much after heat storage and illumination, indicating that the storage stability is good under high temperature and illumination, while the viscosity of Comparative Examples 1-3 is significantly reduced, and the storage stability is poor.
[0067] From the rheological results of the embodiments and comparative examples before and after heat storage and illumination in the attached drawings and Table 1, it can be seen that the low shear viscosity and shear factor of the comparative example change significantly, while the viscosity of the embodiments does not change substantially, indicating that the storage stability is good under high temperature and illumination, and the shear factor changes by <±5% in 10 days under 50°C water bath and UVA-340 lamp irradiation. It is further explained that the polyurea resin provided by the present invention, which is formed by synthesizing polyurea crystals with primary amino-containing benzotriazole as raw material and diisocyanate, not only effectively improves the anti-sagging performance in the initial stage, but also significantly enhances the aging resistance of the resin and prolongs its long-term service life.
[0068] The embodiments of the present invention are described in detail above in conjunction with the accompanying drawings, but the present invention is not limited to the above embodiments. Even if various changes are made to the present invention, if these changes fall within the scope of the claims of the present invention and their equivalents, they still fall within the protection scope of the present invention.
Claims
1. A benzotriazole modified anti-sagging resin, characterized in that: Calculated by weight, it includes the following components:
2. The benzotriazole modified anti-sagging resin according to claim 1, characterized in that: The chemical structure of the primary amino-containing benzotriazole is: Where R 1 —R 8 It is any one of the structures of -H, -OH, -OCH3, -C4H9, -Cl, -CH2NH2, -CH(CH3)3 and -OCH2CHOCH2, or any combination thereof.
3. The benzotriazole-modified anti-sagging resin according to claim 2, characterized in that: The chemical structure of the primary amino-containing benzotriazole is:
4. The benzotriazole modified anti-sagging resin according to claim 1, characterized in that: The solvent is any one or more of xylene, S-100A high boiling point solvent or S-150 aromatic hydrocarbon solvent.
5. The benzotriazole modified anti-sagging resin according to claim 4, characterized in that: When the solvent is a mixed solvent of any two of xylene, S-100A high boiling point solvent or S-150 aromatic hydrocarbon solvent, the arbitrary blending ratio is 1:0-10.
6. The benzotriazole modified anti-sagging resin according to claim 1, characterized in that: The polymer resin is polyacrylic acid resin and / or polyester resin.
7. The benzotriazole modified anti-sagging resin according to claim 1, characterized in that: The diisocyanate is any one of hexamethylene diisocyanate, diphenylmethane-4,4'-diisocyanate or 4,4'-dicyclohexylmethane diisocyanate or a mixture of several of them.
8. A method for preparing the benzotriazole modified anti-sagging resin according to any one of claims 1 to 7, characterized in that: The steps include: S1: mixing primary aminobenzotriazole with part of the solvent to prepare a primary aminobenzotriazole solution of a preset concentration; S2: The polymer resin and the remaining solvent are mixed evenly in a reaction kettle and stirred continuously, the temperature of the reaction system is maintained at 0-40° C., the primary aminobenzotriazole solution prepared in step S1 is dispersed into the reaction system, and diisocyanate is added and stirred to obtain the modified anti-sagging resin.
9. A coating, characterized in that: The invention comprises the benzotriazole modified anti-sagging resin according to any one of claims 1 to 7.