Temperature-resistant silicone rubber compound and preparation method thereof
By introducing ferrocene-based silane-modified silica into silicone rubber, the problem of easy oxidation of silicone rubber at high temperatures was solved, thereby improving its heat oxidation resistance and enhancing its material stability.
Patent Information
- Application Number
- CN202411248063.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-06
- Publication Date
- 2024-11-08
AI Technical Summary
Existing silicone rubber is easily oxidized at high temperatures, leading to a decline in mechanical properties. Ferrocene compounds are also prone to volatilization, affecting their heat resistance and oxidation resistance.
By introducing ferrocene-based silane-modified silica into silicone rubber, the antioxidant properties of the ferrocene group are utilized, and it is stably linked to the surface of silica to avoid volatility issues, thus forming a heat-resistant silicone rubber composite.
It significantly improves the heat and oxidation resistance of silicone rubber, maintains mechanical properties at high temperatures, avoids the volatility problem of ferrocene compounds, and enhances the stability and mechanical properties of the material.
Smart Images

Figure BDA0005031431700000061
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polymer materials, and in particular to a temperature-resistant silicone rubber compound and a preparation method thereof. Background Art
[0002] Silicone rubber is an important polymer material that has been widely used in many fields due to its excellent heat resistance, weather resistance, electrical insulation and biocompatibility. Traditional silicone rubber is usually cross-linked through a vulcanization process to give it elasticity and stability.
[0003] High temperature resistance is one of the most important properties of silicone rubber, so it is used in various high temperature resistant environments. Silicone rubber will oxidize during high temperature use, destroying its mechanical properties. In the presence of oxygen, when the temperature rises to above 250°C, the side methyl groups of silicone rubber will undergo rapid oxidation degradation. First, the silyl methyl group is oxidized to a peroxide group, and then a molecule of formaldehyde is eliminated to generate a silanol group. The generated silanol group further condenses to crosslink the polymer. Ferrocene, as a silicone rubber additive resistant to heat and oxygen aging, has a good inhibitory effect on oxidation USP2979482, but ferrocene and its compounds are easy to sublimate or volatilize, causing contamination of ferrocene and its compounds and reducing the heat and oxidation resistance of silicone rubber. The presence of iron core in ferrocene compounds has a good anti-thermal oxidation effect on polydimethylsiloxane (PDMS), but its high temperature sublimation limits its application in high temperature anti-oxidation of silicone rubber.
[0004] How to solve the above technical problems is the subject faced by the present invention. Summary of the invention
[0005] In order to solve the deficiencies of the prior art, the present invention provides a temperature-resistant silicone rubber compound and a preparation method thereof.
[0006] The technical solution adopted by the present invention to solve the technical problem is: the present invention provides a method for preparing a temperature-resistant silicone rubber compound, comprising the following steps:
[0007] A. Synthesis of ferrocene monolithium salt: Add ferrocene and tetrahydrofuran into a dry 500 ml three-necked flask under nitrogen protection, and stir thoroughly until ferrocene is completely dissolved;
[0008] The solution was cooled to 0°C, tert-butyl lithium was added, cold n-hexane was quickly added to the system after the addition was completed, the system was cooled to below -60°C, and kept for 20 minutes, an orange precipitate appeared;
[0009] The upper solution was removed, and the precipitate was washed with n-hexane for 3 times until the washing solution was colorless, and the solvent was removed to obtain an orange powdery solid, which was the monosubstituted ferrocenium lithium salt;
[0010] B. Synthesis of ferrocenyl chlorosilane: Under nitrogen protection, add the monosubstituted ferrocenyl lithium salt prepared in step A and tetrahydrofuran into a dry three-necked flask and stir until completely dissolved;
[0011] The temperature was lowered to 0°C, and a THF solution of chlorosilane was slowly added to the solution. The mixture was stirred at room temperature overnight. After the solvent and unreacted chlorosilane were removed under reduced pressure, n-hexane was added to extract the product. The n-hexane was removed under reduced pressure to obtain the product ferrocenyl chlorosilane.
[0012] C. Preparation of ferrocenylsilane-modified silica: reacting the ferrocenylsilyl chloride obtained in step B with silica and toluene at 100° C., blowing nitrogen into the reaction process to remove the generated HCl;
[0013] After the reaction is completed, the temperature is cooled to room temperature and water is added twice for washing until the solution is neutral;
[0014] Then, the toluene is extracted under vacuum, and the residue obtained is ferrocenylsilane-modified silica;
[0015] D. Preparation of heat-resistant silicone rubber composite: 5-15 g of ferrocenylsilane-modified silica obtained in step C, 10-20 g of silica, 60-70 g of siloxane, 4-5 g of ethyl orthosilicate and 0.1-0.3 g of dibutyltin dilaurate are mixed evenly on a three-roll mill, then poured into a mold for vacuuming to remove bubbles, and cured at room temperature for 7 days to obtain a heat-resistant silicone rubber composite.
[0016] The amount of ferrocene added is 18-22 g, and the amount of tetrahydrofuran is 110-130 ml;
[0017] Add 28-32 ml of THF solution containing 0.045-0.05 mol tert-butyl lithium over a period of 15-25 minutes;
[0018] The amount of n-hexane added is 110-130ml.
[0019] 8-11 g of the monosubstituted ferrocene lithium salt in step B and 110-130 ml of tetrahydrofuran are stirred until completely dissolved;
[0020] Slowly add 140-160 ml of THF solution of chlorosilane to the solution over a period of 50-70 minutes;
[0021] The solvent and unreacted chlorosilane were removed under reduced pressure, and 40-60 ml of n-hexane was added to extract the product.
[0022] In step C, 12-18 g of ferrocenyl chlorosilane is reacted with 45-55 g of silicon dioxide and 90-110 g of toluene at 95-105° C. for 5-7 hours.
[0023] The chlorosilane in step B is dimethylchlorosilane and / or methylphenylchlorosilane.
[0024] The added amount of the ferrocenylsilane-modified silicon dioxide is 2%-15% of the total mass of the silicone rubber compound.
[0025] The siloxane is hydroxyl-terminated polydimethylsiloxane.
[0026] A heat-resistant silicone rubber compound prepared by the above preparation method.
[0027] The beneficial effects of the present invention are as follows: the present solution connects ferrocenylsilane to the surface of silica, and then adds the modified silica to the vulcanized silicone rubber, thereby significantly improving the heat and oxidation resistance of the silicone rubber. This modification process not only effectively avoids the volatility problem of ferrocene, but also achieves a significant improvement in the overall performance of the material.
[0028] Without the addition of ferrocenylsilane-modified silica, silicone rubber will experience significant performance degradation after thermal oxidative aging, usually manifested as a loss of mechanical properties. This is because the molecular chains of silicone rubber are prone to breakage and oxidation reactions under the combined effects of high temperature and oxygen, resulting in a rapid decrease in the strength and elasticity of the material, thereby losing its proper mechanical properties. This problem is very common in the actual application of silicone rubber, especially when exposed to high temperature environments for a long time, its performance decays rapidly, limiting its service life in high temperature environments.
[0029] In contrast, silicone rubber with ferrocenylsilane-modified silica showed significant resistance to thermal oxidative aging under the same conditions. After thermal oxidative aging, the silicone rubber prepared by this scheme still maintained a high tensile strength, indicating that it can still maintain good mechanical properties at high temperatures. This performance improvement is mainly attributed to the introduction of ferrocenyl groups. Due to its unique structure, ferrocenyl groups have excellent antioxidant properties, which can effectively prevent the oxidation chain reaction initiated by free radicals and reduce the oxidative degradation rate of silicone rubber at high temperatures, thereby delaying the aging process of the material. In addition, ferrocenylsilane is stably connected to the surface of white carbon black through chemical bonds, avoiding the volatility of ferrocenium, enabling it to continue to play an antioxidant role under high temperature conditions, further enhancing the stability of the material.
[0030] Compared with directly adding ferrocene compounds to silicone rubber, this solution not only improves the antioxidant properties, but also overcomes the problem of ferrocene compounds being easy to volatilize. This volatility will not only lead to the attenuation of material performance, but may also cause other safety issues. By connecting ferrocenylsilane to the surface of silica, it not only ensures the stability of the ferrocenyl group in a high temperature environment, but also further enhances the mechanical properties of the material through synergistic effects with silica. As a commonly used inorganic filler, silica has high surface activity and excellent reinforcement effect, which can effectively improve the strength, modulus and wear resistance of silicone rubber. The introduction of ferrocenylsilane not only gives silica excellent antioxidant properties, but also enables the modified silica to be better dispersed in the silicone rubber matrix, forming a more uniform composite material structure with silicone rubber, thereby achieving an improvement in overall performance. DETAILED DESCRIPTION
[0031] In order to clearly illustrate the technical features of this solution, this solution is described below through specific implementation methods.
[0032] Embodiment 1
[0033] This embodiment is a method for preparing a heat-resistant silicone rubber compound, comprising the following steps:
[0034] A. Synthesis of ferrocene monolithium salt: Add 20g ferrocene and 120ml tetrahydrofuran into a dry 500ml three-necked flask under nitrogen protection, and stir thoroughly until the ferrocene is completely dissolved;
[0035] The solution was cooled to 0°C, and 30 ml of THF solution containing 0.048 mol of tert-butyl lithium was added for 20 minutes. After the addition was completed, 120 ml of cold n-hexane was quickly added to the system, and the system was cooled to below -60°C and kept for 20 minutes until an orange precipitate appeared.
[0036] The upper solution was removed, and the precipitate was washed with n-hexane for 3 times until the washing solution was colorless, and the solvent was removed to obtain an orange powdery solid, which was the monosubstituted ferrocenium lithium salt;
[0037] B. Synthesis of ferrocenyl chlorosilane: Under nitrogen protection, add 9.6 g of the monosubstituted ferrocenyl lithium salt obtained in step A and 120 ml of tetrahydrofuran into a dry 50 ml three-necked flask, and stir until completely dissolved;
[0038] The temperature was lowered to 0°C, and 150 ml of a THF solution containing 19.1 g of methylphenyldichlorosilane was slowly added to the solution for 1 hour. The solution was stirred at room temperature overnight, and the solvent and unreacted chlorosilane were removed under reduced pressure. 50 ml of n-hexane was added to extract the product, and the n-hexane was removed under reduced pressure to obtain the product ferrocenyl chlorosilane.
[0039] C. Preparation of ferrocenylsilane-modified silica: 16.1 g (0.045 mol) ferrocenylmethylphenylchlorosilane was reacted with 50 g silica and 100 g toluene at 100° C. for 6 hours. Nitrogen was introduced during the reaction to remove the generated HCl.
[0040] After the reaction is completed, the temperature is cooled to room temperature and water is added twice for washing until the solution is neutral;
[0041] Then, the toluene is extracted under vacuum, and the residue obtained is ferrocenylsilane-modified silica;
[0042] D. Preparation of heat-resistant silicone rubber composite: 15 g of ferrocenylmethylphenylsilane-modified silica obtained in step C, 10 g of silica, 70 g of hydroxyl-terminated polydimethylsiloxane, 4.8 g of ethyl orthosilicate and 0.2 g of dibutyltin dilaurate were mixed evenly on a three-roll mill, then poured into a mold for vacuuming to remove bubbles, and cured at room temperature for 7 days to obtain a heat-resistant silicone rubber composite.
[0043] A heat-resistant silicone rubber compound prepared by the above preparation method.
[0044] Embodiment 2
[0045] This embodiment is a method for preparing a heat-resistant silicone rubber compound, comprising the following steps:
[0046] A. Synthesis of ferrocene monolithium salt: Add 20g ferrocene and 120ml tetrahydrofuran into a dry 500ml three-necked flask under nitrogen protection, and stir thoroughly until the ferrocene is completely dissolved;
[0047] The solution was cooled to 0°C, and 30 ml of THF solution containing 0.048 mol of tert-butyl lithium was added for 20 minutes. After the addition was completed, 120 ml of cold n-hexane was quickly added to the system, and the system was cooled to below -60°C and kept for 20 minutes until an orange precipitate appeared.
[0048] The upper solution was removed, and the precipitate was washed with n-hexane for 3 times until the washing solution was colorless, and the solvent was removed to obtain an orange powdery solid, which was the monosubstituted ferrocenium lithium salt;
[0049] B. Synthesis of ferrocenyl chlorosilane: Under nitrogen protection, add 9.6 g of the monosubstituted ferrocenyl lithium salt obtained in step A and 120 ml of tetrahydrofuran into a dry 50 ml three-necked flask, and stir until completely dissolved;
[0050] The temperature was lowered to 0°C, and 150 ml of a THF solution containing 19.1 g of methylphenyldichlorosilane was slowly added to the solution for 1 hour. The solution was stirred at room temperature overnight, and the solvent and unreacted chlorosilane were removed under reduced pressure. 50 ml of n-hexane was added to extract the product, and the n-hexane was removed under reduced pressure to obtain the product ferrocenyl chlorosilane.
[0051] C. Preparation of ferrocenylsilane-modified silica: 16.1 g (0.045 mol) of ferrocenylmethylphenylchlorosilane was reacted with 50 g of silica and 100 g of toluene at 100° C. for 6 hours. During the reaction, nitrogen was introduced to remove the generated HCl.
[0052] After the reaction is completed, the temperature is cooled to room temperature and water is added twice for washing until the solution is neutral;
[0053] Then, the toluene is extracted under vacuum, and the residue obtained is ferrocenylsilane-modified silica;
[0054] D. Preparation of heat-resistant silicone rubber composite: 5 g of ferrocenylmethylphenylsilane-modified silica, 20 g of silica, 70 g of hydroxyl-terminated polydimethylsiloxane, 4.8 g of ethyl orthosilicate and 0.2 g of dibutyltin dilaurate were mixed evenly on a three-roll mill, then poured into a mold for vacuuming to remove bubbles, and cured at room temperature for 7 days to obtain a heat-resistant silicone rubber composite.
[0055] Embodiment 3
[0056] This embodiment is a method for preparing a heat-resistant silicone rubber compound, comprising the following steps:
[0057] A. Synthesis of ferrocene monolithium salt: Add 20g ferrocene and 120ml tetrahydrofuran into a dry 500ml three-necked flask under nitrogen protection, and stir thoroughly until the ferrocene is completely dissolved;
[0058] The solution was cooled to 0°C, and 30 ml of THF solution containing 0.048 mol of tert-butyl lithium was added for 20 minutes. After the addition was completed, 120 ml of cold n-hexane was quickly added to the system, and the system was cooled to below -60°C and kept for 20 minutes until an orange precipitate appeared.
[0059] The upper solution was removed, and the precipitate was washed with n-hexane for 3 times until the washing solution was colorless. The solvent was removed to obtain an orange powdery solid, which was the monosubstituted ferrocenium lithium salt;
[0060] B. Synthesis of ferrocenyl chlorosilane: Under nitrogen protection, add 9.6 g of the monosubstituted ferrocenyl lithium salt obtained in step A and 120 ml of tetrahydrofuran into a dry 50 ml three-necked flask, and stir until completely dissolved;
[0061] The temperature was lowered to 0°C, and 150 ml of a THF solution containing 12.9 g of dimethyldichlorosilane was slowly added to the solution for 1 hour. The solution was stirred at room temperature overnight, and the solvent and unreacted chlorosilane were removed under reduced pressure. 50 ml of n-hexane was added to extract the product, and the n-hexane was removed under reduced pressure to obtain the product ferrocenyl chlorosilane.
[0062] C. Preparation of ferrocenylsilane-modified silica: 13.9 g of ferrocenyldimethylsilyl chloride, 50 g of silica, and 100 g of toluene were reacted at 100° C. for 6 hours. During the reaction, nitrogen was blown in to remove the generated HCl.
[0063] After the reaction is completed, the temperature is cooled to room temperature and water is added twice for washing until the solution is neutral;
[0064] Then, the toluene is extracted under vacuum, and the residue obtained is ferrocenyldimethylsilane-modified silica;
[0065] D. Preparation of heat-resistant silicone rubber composite: 15 g of ferrocenyldimethylsilane-modified silica, 10 g of silica, 70 g of hydroxyl-terminated polydimethylsiloxane, 4.8 g of ethyl orthosilicate and 0.2 g of dibutyltin dilaurate were mixed evenly on a three-roll mill, then poured into a mold for vacuuming to remove bubbles, and cured at room temperature for 7 days to obtain a heat-resistant silicone rubber composite.
[0066] Comparative Example 1
[0067] This comparative example is a method for preparing a silicone rubber composite. 25 g of silicon dioxide, 70 g of hydroxyl-terminated polydimethylsiloxane, 4.8 g of ethyl orthosilicate and 0.2 g of dibutyltin dilaurate are mixed evenly on a three-roll mill, then poured into a mold for vacuuming to remove bubbles, and cured at room temperature for 7 days to obtain a heat-resistant silicone rubber composite.
[0068] The prepared silicone rubber composite was cut into dumbbell-shaped specimens according to the national standard GB528-98, and a room temperature tensile test was performed on an Instron 5565 universal electronic material testing machine, with a length between the clamps of 10 mm and a tensile rate of 200 mm / min.
[0069] Hot air aging: the aging temperature is 250℃, the aging time is 72h, and the atmosphere is air.
[0070] Table 1 Mechanical properties test data
[0071]
[0072] It can be seen from Table 1 that the silicone rubber without ferrocenylsilane-modified silica has lost its mechanical properties after thermal oxidative aging. However, the silicone rubber with ferrocenylsilane-modified silica still maintains good tensile strength, indicating that it has good thermal oxidative aging resistance.
[0073] The initial tensile strength of Example 1 and Example 2 is 1.3 MPa, while the initial tensile strength of Example 3 and Comparative Example 1 is 1.2 MPa. It can be seen that Example 1 and Example 2 have good initial mechanical properties before aging treatment. In comparison, Example 3 and Comparative Example 1 are slightly inferior, but the difference is not large.
[0074] The tensile strength of Example 1 dropped to 0.9MPa after thermal oxidative aging. Despite aging at 250°C for 72 hours, the composite still maintained 69% of its original tensile strength. The tensile strength of Example 2 after thermal oxidative aging was 0.6MPa, maintaining 46% of its original tensile strength. Compared with Example 1, although the initial tensile strength was the same, its performance after thermal oxidative aging decreased significantly. This is because the added ferrocenylsilane-modified silica was reduced, which weakened its resistance to thermal oxidative aging. The tensile strength of Example 3 after thermal oxidative aging was 0.8MPa, maintaining 67% of its original tensile strength. Similar to Example 1, it can be seen that the performance of the composite after thermal oxidative aging is relatively stable.
[0075] Comparative Example 1 has completely lost its mechanical properties after thermal oxidative aging, which indicates that the silicone rubber without the addition of ferrocenylsilane-modified silica has poor tolerance under high temperature aging environment.
[0076] Both Examples 1 and 3 performed relatively well after thermal oxidative aging, maintaining 69% and 67% of the original tensile strength, respectively. This shows that ferrocenyldimethylsilane-modified silica has a significant effect in improving the thermal oxidation resistance of silicone rubber. Example 1 is slightly better than Example 3 because the phenyl group in different ferrocenylsilanes has a better antioxidant effect than the methyl group. The tensile strength of Example 2 decreased significantly after thermal oxidative aging, and only 46% of the initial strength was maintained. This is because the amount of ferrocenylsilane added was reduced, making its antioxidant performance inferior to that of Examples 1 and 3, so the stability of the material at high temperatures is relatively poor.
[0077] Technical features not described in the present invention can be achieved through or by adopting existing technologies and will not be described in detail here. Of course, the above description is not a limitation of the present invention, and the present invention is not limited to the above examples. Changes, modifications, additions or substitutions made by ordinary technicians in this technical field within the essential scope of the present invention should also fall within the scope of protection of the present invention.
Claims
1. A method for preparing a heat-resistant silicone rubber compound, characterized in that: The following steps are included: A. Synthesis of ferrocene monolithium salt: Under nitrogen protection, ferrocene and tetrahydrofuran were mixed and stirred until completely dissolved; After the solution was cooled to 0°C, tert-butyl lithium was added, followed by rapid addition of cold n-hexane, and the system was cooled to below -60°C for 20 minutes, and an orange precipitate appeared; After removing the upper solution, the precipitate was washed with n-hexane three times and dried to obtain orange powdery monosubstituted ferrocenium lithium salt; B. Synthesis of ferrocenyl chlorosilane: Under nitrogen protection, dissolve monosubstituted ferrocenyl lithium salt in tetrahydrofuran, cool to 0°C, slowly add THF solution of chlorosilane, and stir at room temperature overnight; The solvent and unreacted chlorosilane are removed under reduced pressure, n-hexane is added to extract the product, and the n-hexane is removed under reduced pressure to obtain ferrocenyl chlorosilane; C. Preparation of ferrocenylsilane-modified silica: reacting the ferrocenylsilyl chloride obtained in step B with silica and toluene at 100° C., blowing nitrogen into the reaction process to remove the generated HCl; After the reaction is completed, the temperature is cooled to room temperature and water is added twice for washing until the solution is neutral; Then, the toluene is extracted under vacuum, and the residue obtained is ferrocenylsilane-modified silica; D. Preparation of heat-resistant silicone rubber composite: The ferrocenylsilane-modified silica, silica, siloxane, ethyl orthosilicate and dibutyltin dilaurate prepared in step C are uniformly mixed on a three-roll mill, then poured into a mold for vacuuming to remove bubbles, and cured at room temperature to obtain a heat-resistant silicone rubber composite.
2. The method for preparing the heat-resistant silicone rubber compound according to claim 1, characterized in that: In step A, the amount of ferrocene added is 18-22 g, and the amount of tetrahydrofuran is 110-130 ml; The amount of n-hexane added is 110-130ml.
3. The method for preparing the heat-resistant silicone rubber compound according to claim 1, characterized in that: In step A, 28-32 ml of a THF solution containing 0.045-0.05 mol of tert-butyl lithium is added, and the addition time is 15-25 minutes.
4. The method for preparing the heat-resistant silicone rubber compound according to claim 1, characterized in that: In step B, 8-11 g of lithium monosubstituted ferrocenium salt and 110-130 ml of tetrahydrofuran are stirred until completely dissolved.
5. The method for preparing the heat-resistant silicone rubber compound according to claim 1, characterized in that: In step B, 140-160 ml of THF solution of chlorosilane is slowly added over 50-70 minutes; The solvent and unreacted chlorosilane were removed under reduced pressure, and 40-60 ml of n-hexane was added to extract the product.
6. The method for preparing the heat-resistant silicone rubber compound according to claim 1, characterized in that: In step C, 12-18 g of ferrocenyldichlorosilane is reacted with 45-55 g of silicon dioxide and 90-110 g of toluene at 95-105° C. for 5-7 hours.
7. The method for preparing the heat-resistant silicone rubber compound according to claim 1, characterized in that: The chlorosilane in step B is dimethylchlorosilane and / or methylphenylchlorosilane.
8. The method for preparing the heat-resistant silicone rubber compound according to claim 1, characterized in that: The added amount of the ferrocenylsilane-modified silicon dioxide is 2%-15% of the total mass of the silicone rubber compound.
9. The method for preparing the heat-resistant silicone rubber compound according to claim 1, characterized in that: The siloxane is hydroxyl-terminated polydimethylsiloxane.
10. A heat-resistant silicone rubber composite prepared by the preparation method according to any one of claims 1 to 9.