MXene modified polyaspartic acid ester as well as preparation method and application thereof

Through the preparation of MXene modified polyaspartic acid ester, the problem of poor hydrophobicity and salt spray corrosion resistance in polyurea coatings is solved, and high-performance coating corrosion protection and mechanical strength improvement is achieved, suitable for engineering machinery protection and Marine anti-corrosion field.

CN118909250APending Publication Date: 2024-11-08JIANGSU FUQISEN NEW MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411135202.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing polyaspartic acid ester has poor hydrophobicity, adhesion and salt spray corrosion resistance in polyurea coatings, which limits its application in the fields of engineering machinery protection and marine corrosion protection.

Method used

Using the preparation method of MXene modified polyaspartic acid ester, the silane coupling agent and MXene powder react under ultrasonic and stirring to form MXene-NH2 and perform addition reaction with dihydrocarbon maleate. , construct a hybrid structure of two-dimensional inorganic materials and organic polymers to form a high-performance MXene modified polyaspartic acid ester.

Benefits of technology

The corrosion resistance and mechanical properties of PAE polyurea coatings have been significantly improved, the corrosion resistance and adhesion of the coating have been enhanced, especially the salt spray resistance has been significantly improved, and the tensile strength has also been significantly improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118909250A_ABST
    Figure CN118909250A_ABST
Patent Text Reader

Abstract

The invention provides MXene modified polyaspartic acid ester as well as a preparation method and application thereof, and belongs to the technical field of high-performance polyurea coatings. The preparation method comprises the following steps: adding a silane coupling agent-ethanol solution into an MXene aqueous solution, carrying out ultrasonic treatment, stirring, adding a hydrochloric acid solution, adjusting the pH value, and carrying out a reaction to obtain MXene-NH2; then, dihydrocarbon maleate is dropwise added into MXene-NH2 to be subjected to an addition reaction, and MXene modified polyaspartic acid ester is obtained; finally, the prepared MXene modified polyaspartic acid ester and an isocyanate curing agent are mixed in butyl acetate, and the MXene modified polyaspartic acid ester polyurea coating is obtained. The MXene modified polyaspartic acid ester prepared by the preparation method disclosed by the invention can be used for remarkably improving the corrosion resistance and the mechanical property of the polyurea coating. The preparation method disclosed by the invention is simple, rapid, easy to operate and wider in application.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of high-performance polyurea coatings, and in particular to a MXene-modified polyaspartic acid ester and a preparation method and application thereof. Background Art

[0002] Polyurea coating is an elastic coating material made by reacting amino components with isocyanates. Polyurea coating has many advantages such as fast curing speed, low viscosity, high mechanical properties, and low solvent content. It has been widely used in steel structures, vehicle engineering, equipment parts, wind turbine blades, concrete and other fields. However, traditional polyurea coatings have a fast curing speed and require special spraying equipment. In addition, its construction gel time is short and its stability is poor, which limits its promotion and application to a certain extent. The polyaspartic acid ester polyurea coating prepared using polyaspartic acid ester (PAE) as the amino component has the characteristics of adjustable gel time, long-term outdoor use, and better comprehensive performance. Therefore, PAE polyurea coating, as the third generation of polyurea, has been used in more fields, and the market demand is on an upward trend.

[0003] PAE polyurea coating is a new type of polyurea coating generated by the reaction of isocyanate and polyaspartic acid ester (PAE) containing amino functional groups. PAE is actually a sterically hindered aliphatic secondary amine compound. Its preparation principle is based on the Michael addition reaction, which uses aliphatic primary amines to react with unsaturated maleic acid dialkyl esters to generate aliphatic secondary amine compounds with sterically hindered structures. It is precisely because of its unique steric hindrance effect that it can limit the reaction between isocyanate and amino groups and reduce their reactivity, thereby further increasing the gel time of polyurea. Compared with the previous two generations of polyurea products, the gel time of PAE polyurea can reach tens of hours, which greatly reduces the construction cost and improves the convenience of construction. However, due to the introduction of amine hydrophilic groups in the preparation process of PAE polyurea, the coating has poor hydrophobicity, easy moisture absorption, and poor thermal performance. In addition, due to the low conversion rate of primary amines during its synthesis, the reaction is difficult to be completely carried out, resulting in insufficient curing in the later stage. Therefore, compared with the first two generations of traditional polyurea, the adhesion of the cured PAE polyurea coating is slightly insufficient and its salt spray corrosion resistance is poor, which to a certain extent limits its application in engineering machinery protection and marine corrosion protection.

[0004] In view of this, the present invention proposes for the first time a MXene-modified polyaspartic acid ester with good adhesion, hydrophobicity and salt spray corrosion resistance. Summary of the invention

[0005] The object of the present invention is to provide a MXene-modified polyaspartic acid ester and a preparation method and application thereof, so as to solve the technical problems in the prior art that polyaspartic acid ester has poor hydrophobicity, adhesion and salt spray corrosion resistance in polyurea coatings.

[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0007] The present invention provides a method for preparing MXene-modified polyaspartic acid ester, comprising the following steps:

[0008] (1) adding a silane coupling agent-ethanol solution to a MXene aqueous solution, performing ultrasonication and stirring, and then adding a hydrochloric acid solution to adjust the pH and react to obtain MXene-NH2;

[0009] (2) Maleic acid dialkyl ester is added dropwise to MXene-NH2 for addition reaction to obtain MXene-modified polyaspartic acid ester.

[0010] Furthermore, the MXene aqueous solution is obtained by dissolving MXene powder in water;

[0011] The silane coupling agent-ethanol solution is obtained by dispersing the silane coupling agent in ethanol;

[0012] The volume ratio of water to ethanol is 500-1000:300-600;

[0013] The mass ratio of the MXene powder to the silane coupling agent is 3-8:8-16;

[0014] The mass volume ratio of the MXene powder and water is 3-8 g:500-1000 mL.

[0015] Furthermore, the MXene powder is Ti3C2T x , where T x represents the chemical functional groups on the MXene surface;

[0016] The silane coupling agent includes one or more of KH550, KH792 and DL602;

[0017] The maleic acid dihydrocarbon ester includes one or more of dimethyl maleate, diethyl maleate, dibutyl maleate, dioctyl maleate, diisooctyl maleate and diallyl maleate.

[0018] Furthermore, in step (1), the ultrasonication time is 30 to 60 minutes, and the stirring time is 10 to 20 minutes;

[0019] The pH value is adjusted to 4-5;

[0020] The molar concentration of the hydrochloric acid solution is 0.5-2 mol / L.

[0021] Furthermore, in the step (1), the reaction temperature is 30 to 50° C., and the reaction time is 8 to 24 hours.

[0022] Furthermore, in the step (2), the mass ratio of MXene-NH2 to dialkyl maleate is 10-18:3.5-5.5.

[0023] Furthermore, in the step (2), the dropping temperature is 50 to 70° C., and the dropping time is 20 to 50 min;

[0024] The temperature of the addition reaction is 90-120° C., and the time of the addition reaction is 10-30 minutes.

[0025] The present invention provides a MXene-modified polyaspartic acid ester prepared by a preparation method of a MXene-modified polyaspartic acid ester.

[0026] The present invention also provides an application of MXene-modified polyaspartic acid ester in preparing a polyurea coating, wherein the MXene-modified polyaspartic acid ester and an isocyanate curing agent are mixed in butyl acetate to obtain a MXene-modified polyaspartic acid ester polyurea coating;

[0027] The isocyanate curing agent is a solvent-based isocyanate oligomer.

[0028] Furthermore, the mass ratio of the MXene-modified polyaspartic acid ester to the isocyanate curing agent is 14-20:5-15;

[0029] The amount of butyl acetate used is 10 to 50% of the total mass of the MXene-modified polyaspartic acid ester and the isocyanate curing agent.

[0030] Beneficial effects of the present invention:

[0031] (1) The preparation method of the present invention treats the MXene-NH2 after grafting with silane coupling agent as a primary amine substance, and carries out an addition reaction with dialkyl maleate. For the first time, MXene is grafted into polyaspartic acid ester by a chemical method, and an effective hybridization of two-dimensional inorganic materials and polyaspartic acid ester organic polymers is successfully constructed to obtain a high-performance MXene-modified polyaspartic acid ester polyurea coating.

[0032] (2) Due to the repulsive force of the polymer chain segments, the MXene sheets are difficult to stack on each other, which ensures that the microstructure of the MXene "maze effect" is not destroyed, effectively exerts the shielding effect of MXene, and significantly improves the anti-corrosion performance of PAE polyurea coatings.

[0033] (3) The preparation method of the present invention not only improves the corrosion resistance of the polyurea coating by grafting MXene as a reinforcing phase into the polyurea coating, but also gives the coating excellent mechanical properties, thereby further increasing the mechanical strength of the polyurea paint film.

[0034] (4) The preparation method of the present invention is simple, fast, easy to operate and popularize. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 This is the infrared spectrum of MXene-NH2 prepared in Example 1 of the present invention;

[0036] Figure 2 It is a schematic diagram of the reaction process in the preparation method of the present invention. DETAILED DESCRIPTION

[0037] The present invention provides a method for preparing MXene-modified polyaspartic acid ester, comprising the following steps:

[0038] (1) adding a silane coupling agent-ethanol solution to a MXene aqueous solution, performing ultrasonication and stirring, and then adding a hydrochloric acid solution to adjust the pH and react to obtain MXene-NH2;

[0039] (2) Maleic acid dialkyl ester is added dropwise to MXene-NH2 for addition reaction to obtain MXene-modified polyaspartic acid ester.

[0040] In the present invention, the MXene aqueous solution is obtained by dissolving MXene powder in water;

[0041] The silane coupling agent-ethanol solution is obtained by dispersing the silane coupling agent in ethanol.

[0042] In the present invention, the volume ratio of water to ethanol is 500-1000:300-600, preferably 530-990:350-580, and more preferably 560-980:400-550;

[0043] The mass ratio of the MXene powder to the silane coupling agent is 3-8:8-16, preferably 3.4-7.5:8.5-15.5, and more preferably 3.6-7.2:9-15;

[0044] The mass volume ratio of the MXene powder and water is 3-8 g:500-1000 mL, preferably 3.4-7.5 g:530-990 mL, and more preferably 3.6-7.2 g:560-980 mL.

[0045] In the present invention, the MXene powder is Ti3C2T x , where Tx Represents the chemical functional groups on the MXene surface.

[0046] In the present invention, the silane coupling agent includes one or more of KH550, KH792 and DL602, preferably KH550 and / or KH792, and more preferably KH550.

[0047] In the present invention, the maleic acid dialkyl ester includes one or more of dimethyl maleate, diethyl maleate, dibutyl maleate, dioctyl maleate, diisooctyl maleate and diallyl maleate, preferably one or more of dimethyl maleate, diethyl maleate, dibutyl maleate, dioctyl maleate and diallyl maleate, and further preferably one or more of dimethyl maleate, diethyl maleate, dioctyl maleate and diallyl maleate.

[0048] In the present invention, in step (1), the ultrasonic time is 30 to 60 minutes, preferably 35 to 55 minutes, and more preferably 40 to 50 minutes;

[0049] The stirring time is 10 to 20 minutes, preferably 12 to 18 minutes, and more preferably 15 minutes.

[0050] In the present invention, the pH is adjusted to 4 to 5, preferably 4.2 to 4.8, and more preferably 4.5.

[0051] In the present invention, the molar concentration of the hydrochloric acid solution is 0.5 to 2 mol / L, preferably 0.8 to 1.5 mol / L, and more preferably 1 mol / L.

[0052] In the present invention, in the step (1), the reaction temperature is 30 to 50°C, preferably 35 to 45°C, and more preferably 40°C; the reaction time is 8 to 24h, preferably 10 to 20h, and more preferably 12 to 18h.

[0053] In the present invention, in step (1), after the reaction is completed, the mixture is cooled to room temperature, washed with deionized water and ethanol to remove unreacted coupling agent, and finally the obtained MXene-NH2 product is dried in a vacuum oven at 40°C.

[0054] In the present invention, in the step (2), the mass ratio of MXene-NH2 to dialkyl maleate is 10-18:3.5-5.5, preferably 12-17:3.75-5.3, and more preferably 15-16:4-5.1.

[0055] In the present invention, in step (2), the dropping temperature is 50-70°C, preferably 55-65°C, and more preferably 60°C; the dropping time is 20-50 min, preferably 25-45 min, and more preferably 30-40 min.

[0056] In the present invention, the temperature of the addition reaction is 90-120° C., preferably 95-115° C., and more preferably 100-110° C.; the time of the addition reaction is 10-30 min, preferably 15-25 min, and more preferably 20 min.

[0057] The reaction mechanism of the present invention is as follows: the amino-containing silane coupling agent will first hydrolyze to form silanol, which reacts with the hydroxyl group on the surface of MXene to form a -Si-O- bond, thereby grafting the -NH2 in the silane coupling agent to the MXene; the MXene after grafting the coupling agent can be regarded as a primary amine substance, which can undergo a Michael addition reaction with dialkyl maleate, and the MXene is grafted onto the polyaspartic acid ester resin through chemical action, forming a structure of MXene grafted modified polyaspartic acid ester, thereby constructing an effective hybridization of two-dimensional inorganic materials and organic polymers.

[0058] The present invention provides a MXene-modified polyaspartic acid ester prepared by a preparation method of a MXene-modified polyaspartic acid ester.

[0059] The present invention also provides an application of MXene-modified polyaspartic acid ester in the preparation of polyurea coatings, wherein the MXene-modified polyaspartic acid ester and an isocyanate curing agent are mixed in butyl acetate to obtain a MXene-modified polyaspartic acid ester polyurea coating.

[0060] In the present invention, the isocyanate curing agent is a solvent-based isocyanate oligomer, preferably TPA-100, N3390, N3300, HI-100 or HT-100, and more preferably TPA-100 or N3390.

[0061] In the present invention, the mass ratio of the MXene-modified polyaspartic acid ester to the isocyanate curing agent is 14-20:5-15, preferably 15-19:5.4-14.5, and more preferably 16-18:6-14.

[0062] In the present invention, the amount of butyl acetate used is 10 to 50% of the total mass of the MXene-modified polyaspartic acid ester and the isocyanate curing agent, preferably 15 to 45%, and more preferably 20 to 30%.

[0063] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.

[0064] Example 1

[0065] 5g Ti3C2T x The powder was dissolved in 800 mL of deionized water to obtain a uniform Ti3C2T x Aqueous solution; 12g of silane coupling agent KH550 was dispersed in 500mL of ethanol and stirred thoroughly to completely dissolve it to obtain a KH550-ethanol solution; then the dispersed KH550-ethanol solution was added to the Ti3C2T x Ultrasonication in aqueous solution for 40 minutes, stirring for 15 minutes; then adding 1 mol / L hydrochloric acid solution to adjust the pH to 5, reacting at 50°C for 24 hours, cooling to room temperature after the reaction, washing with deionized water and ethanol to remove unreacted silane coupling agent, and finally drying in a vacuum oven at 40°C to obtain MXene-NH2;

[0066] The prepared MXene-NH2 was tested, and the test results are as follows Figure 1 shown. Figure 1 This is the infrared spectrum of MXene-NH2 prepared in Example 1 of the present invention. Figure 1 It can be seen that the MXene-NH2 product has been grafted with -NH2 functional groups.

[0067] 15g MXene-NH2 powder was heated to 50°C, and then 3.75g diethyl maleate was dropped into it for 30 minutes. After the addition was completed, the temperature was raised to 100°C for addition reaction for 30 minutes to obtain MXene-modified polyaspartic acid ester, which was recorded as PAE-1.

[0068] The prepared 16 g MXene-modified polyaspartic acid ester PAE-1 and 9.7 g isocyanate curing agent N3390 (N3390 is produced by Covestro AG of Germany) were mixed in 8 g butyl acetate to obtain MXene-modified polyaspartic acid ester polyurea coating PAEC-1.

[0069] PAEC-1 was coated onto tinplate and steel plate using a wire rod coater, dried in a constant temperature and humidity room (23°C, 52% RH), and then cured at room temperature for 7 days for performance testing. The test results are shown in Table 1.

[0070] Example 2

[0071] 4.2g Ti3C2T x The powder was dissolved in 600 mL of deionized water to obtain a uniform Ti3C2T xAqueous solution; 13.8 g of silane coupling agent KH792 was dispersed in 400 mL of ethanol and stirred thoroughly to dissolve it completely to obtain a KH792-ethanol solution; then the dispersed KH792-ethanol solution was added to the Ti3C2T x Ultrasonication in aqueous solution for 30 minutes, stirring for 20 minutes; then adding 1 mol / L hydrochloric acid solution to adjust the pH to 4.5, reacting at 60°C for 12 hours, cooling to room temperature after the reaction, washing with deionized water and ethanol to remove unreacted silane coupling agent, and finally drying in a vacuum oven at 40°C to obtain MXene-NH2;

[0072] 16g MXene-NH2 powder was heated to 50°C, and then 5.1g dimethyl maleate was dropped into it for 30 minutes. After the addition was completed, the temperature was raised to 110°C for addition reaction for 40 minutes to obtain MXene-modified polyaspartic acid ester, which was recorded as PAE-2.

[0073] The prepared 20 g MXene-modified polyaspartic acid ester PAE-2 and 12.8 g isocyanate curing agent TPA-100 (TPA-100 is produced by Asahi Chemical of Japan) were mixed in 6.6 g butyl acetate to obtain MXene-modified polyaspartic acid ester polyurea coating PAEC-2.

[0074] PAEC-2 was coated onto tinplate and steel plate using a wire rod coater, dried in a constant temperature and humidity room (23°C, 52% RH), and then cured at room temperature for 7 days for performance testing. The test results are shown in Table 1.

[0075] Example 3

[0076] 3.6g Ti3C2T x The powder was dissolved in 560 mL of deionized water to obtain a uniform Ti3C2T x Aqueous solution; 8.5 g of silane coupling agent KH550 was dispersed in 300 mL of ethanol and stirred thoroughly to dissolve it completely to obtain a KH550-ethanol solution; then the dispersed KH550-ethanol solution was added to the Ti3C2T x Ultrasonication in aqueous solution for 30 minutes, stirring for 20 minutes; then adding 1 mol / L hydrochloric acid solution to adjust the pH to 5, reacting at 50°C for 24 hours, cooling to room temperature after the reaction, washing with deionized water and ethanol to remove unreacted silane coupling agent, and finally drying in a vacuum oven at 40°C to obtain MXene-NH2;

[0077] 10g MXene-NH2 powder was heated to 60°C, and then 4.8g dioctyl maleate was dropped into it for 30 minutes. After the addition was completed, the temperature was raised to 120°C for addition reaction for 20 minutes to obtain MXene-modified polyaspartic acid ester, which was recorded as PAE-3.

[0078] 14 g of the prepared MXene-modified polyaspartic acid ester PAE-3 and 5.4 g of isocyanate curing agent HI-100 (HI-100 is produced by BASF) were mixed in 5.5 g of butyl acetate to obtain a MXene-modified polyaspartic acid ester polyurea coating PAEC-3.

[0079] PAEC-3 was coated onto tinplate and steel plate using a wire rod coater, dried in a constant temperature and humidity room (23°C, 52% RH), and then cured at room temperature for 7 days for performance testing. The test results are shown in Table 1.

[0080] Example 4

[0081] 7.2g Ti3C2T x The powder was dissolved in 980 mL of deionized water to obtain a uniform Ti3C2T x Aqueous solution; 16 g of silane coupling agent DL602 was dispersed in 600 mL of ethanol and stirred thoroughly to completely dissolve it to obtain a DL602-ethanol solution; then the dispersed DL602-ethanol solution was added to the Ti3C2T x Ultrasonication in aqueous solution for 30 minutes, stirring for 15 minutes; then adding 1 mol / L hydrochloric acid solution to adjust the pH to 4.5, reacting at 60°C for 18 hours, cooling to room temperature after the reaction, washing with deionized water and ethanol to remove unreacted silane coupling agent, and finally drying in a vacuum oven at 40°C to obtain MXene-NH2;

[0082] 18g MXene-NH2 powder was heated to 60°C, and then 4.5g diethyl maleate was dropped into it for 30 minutes. After the addition was completed, the temperature was raised to 110°C for addition reaction for 30 minutes to obtain MXene-modified polyaspartic acid ester, which was recorded as PAE-4.

[0083] 19 g of the prepared MXene-modified polyaspartic acid ester PAE-1 and 8.9 g of isocyanate curing agent HT-100 (the manufacturer of HT-100 is Wanhua Chemical) were mixed in 8.5 g of butyl acetate to obtain a MXene-modified polyaspartic acid ester polyurea coating PAEC-4.

[0084] PAEC-4 was coated onto tinplate and steel plate using a wire rod coater, dried in a constant temperature and humidity room (23°C, 52% RH), and then cured at room temperature for 7 days for performance testing. The test results are shown in Table 1.

[0085] Example 5

[0086] 5.8g Ti3C2T x The powder was dissolved in 850 mL of deionized water to obtain a uniform Ti3C2T x Aqueous solution; 14.5 g of silane coupling agent KH792 was dispersed in 550 mL of ethanol and stirred thoroughly to dissolve it completely to obtain a KH792-ethanol solution; then the dispersed KH792-ethanol solution was added to the Ti3C2T x Ultrasonication in aqueous solution for 30 minutes, stirring for 20 minutes; then adding 1 mol / L hydrochloric acid solution to adjust the pH to 5, reacting at 60°C for 15 hours, cooling to room temperature after the reaction, washing with deionized water and ethanol to remove unreacted silane coupling agent, and finally drying in a vacuum oven at 40°C to obtain MXene-NH2;

[0087] 17g MXene-NH2 powder was heated to 60°C, and then 4.9g dimethyl maleate was dropped into it for 30 minutes. After the addition was completed, the temperature was raised to 100°C for addition reaction for 30 minutes to obtain MXene-modified polyaspartic acid ester, which was recorded as PAE-5.

[0088] The prepared 20 g MXene-modified polyaspartic acid ester PAE-5 and 14.5 g isocyanate curing agent N3390 (N3390 is produced by Covestro AG of Germany) were mixed in 14.5 g butyl acetate to obtain MXene-modified polyaspartic acid ester polyurea coating PAEC-5.

[0089] PAEC-5 was coated onto tinplate and steel plate using a wire rod coater, dried in a constant temperature and humidity room (23°C, 52% RH), and then cured at room temperature for 7 days for performance testing. The test results are shown in Table 1.

[0090] Comparative Example 1

[0091] 1.85 g of isophorone diamine was added to the reaction bottle, the temperature was raised to 50° C., and then 3.75 g of diethyl maleate was dropped in for 30 min. After the dropwise addition was completed, the temperature was raised to 100° C. for addition reaction for 30 min to obtain polyaspartic acid ester, which was recorded as PAE-D1.

[0092] The prepared polyaspartic acid ester PAE-D1 and 5.2 g of isocyanate curing agent N3390 (N3390 is produced by Covestro AG of Germany) were mixed in 4.5 g of butyl acetate to obtain a polyaspartic acid ester polyurea coating PAEC-D1.

[0093] PAEC-D1 was coated onto tinplate and steel plate using a wire rod coater, dried in a constant temperature and humidity room (23°C, 52% RH), and then cured at room temperature for 7 days for performance testing. The test results are shown in Table 1.

[0094] Comparative Example 2

[0095] 2.1 g of 1,6-hexanediamine was added to the reaction bottle, the temperature was raised to 50°C, and then 5.1 g of dimethyl maleate was added dropwise for 30 min. After the addition was completed, the temperature was raised to 110°C for addition reaction for 40 min to obtain polyaspartic acid ester, which was recorded as PAE-D2.

[0096] The prepared polyaspartic acid ester PAE-D2 and 6.6 g of isocyanate curing agent TPA-100 (TPA-100 is produced by Asahi Chemical of Japan) were mixed in 5.8 g of butyl acetate to obtain polyaspartic acid ester polyurea coating PAEC-D2.

[0097] PAEC-D2 was coated onto tinplate and steel plate using a wire rod coater, dried in a constant temperature and humidity room (23°C, 52% RH), and then cured at room temperature for 7 days for performance testing. The test results are shown in Table 1.

[0098] The properties of the paint films of the polyaspartic acid ester polyurea coatings prepared in Examples 1 to 5 and Comparative Examples 1 to 2 after curing were tested, and the test methods for various performance indicators are as follows:

[0099] Pencil hardness test: refer to GB / T 6739-2006;

[0100] Adhesion test: refer to GB / T 9286-1998;

[0101] Impact resistance test: refer to GB / T 1732-2020;

[0102] Tensile strength test: refer to GB / T 528-2009;

[0103] Aging resistance test: refer to GB / T 1865-2009 method 1;

[0104] Salt spray resistance test: refer to GB / T 1771-2007;

[0105] Moisture and heat resistance test: refer to GB / T 1740-2007;

[0106] Acid and alkali resistance test: refer to GB / T 9274-1988 Method A.

[0107] The test results are shown in Table 1.

[0108] Table 1 Performance test results of Examples 1 to 5 and Comparative Examples 1 to 2

[0109]

[0110] As can be seen from the above embodiments, the present invention provides a MXene-modified polyaspartic acid ester and its preparation method and application, wherein a silane coupling agent-ethanol solution is added to a MXene aqueous solution for ultrasonication and stirring, and then a hydrochloric acid solution is added to adjust the pH and then reacted to obtain MXene-NH2; maleic acid dialkyl ester is added dropwise to MXene-NH2 for addition reaction to obtain MXene-modified polyaspartic acid ester; the prepared MXene-modified polyaspartic acid ester and isocyanate curing agent are mixed in butyl acetate to obtain a MXene-modified polyaspartic acid ester polyurea coating. Compared with the comparative example, the salt spray resistance and acid and alkali resistance of the polyaspartic acid ester polyurea coating prepared by the present invention are significantly improved, especially the overall salt spray resistance is significantly improved, up to 3120h, while the salt spray resistance of conventional PAE polyurea coatings that have not been modified by MXene is within 2000h. In addition, the tensile strength of the polyurea coating prepared by the preparation method of the present invention is significantly higher than that of the commercially available product of the comparative example, indicating that the grafting modification of MXene also exerts the high strength characteristics of its two-dimensional material, which can further improve the mechanical strength of the polyurea coating.

[0111] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing MXene-modified polyaspartic acid ester, characterized in that: The following steps are involved: (1) adding a silane coupling agent-ethanol solution to a MXene aqueous solution, performing ultrasonication and stirring, and then adding a hydrochloric acid solution to adjust the pH and react to obtain MXene-NH2; (2) Maleic acid dialkyl ester is added dropwise to MXene-NH2 for addition reaction to obtain MXene-modified polyaspartic acid ester.

2. The method for preparing MXene-modified polyaspartic acid ester according to claim 1, characterized in that: The MXene aqueous solution is obtained by dissolving MXene powder in water; The silane coupling agent-ethanol solution is obtained by dispersing the silane coupling agent in ethanol; The volume ratio of water to ethanol is 500-1000:300-600; The mass ratio of the MXene powder to the silane coupling agent is 3-8:8-16; The mass volume ratio of the MXene powder and water is 3-8 g:500-1000 mL.

3. The method for preparing MXene-modified polyaspartic acid ester according to claim 2, characterized in that: The MXene powder is Ti3C2T x , where T x represents the chemical functional groups on the MXene surface; The silane coupling agent includes one or more of KH550, KH792 and DL602; The maleic acid dihydrocarbon ester includes one or more of dimethyl maleate, diethyl maleate, dibutyl maleate, dioctyl maleate, diisooctyl maleate and diallyl maleate.

4. The method for preparing MXene-modified polyaspartic acid ester according to claim 2 or 3, characterized in that: In the step (1), the ultrasonication time is 30 to 60 minutes, and the stirring time is 10 to 20 minutes; The pH value is adjusted to 4-5; The molar concentration of the hydrochloric acid solution is 0.5-2 mol / L.

5. The method for preparing MXene-modified polyaspartic acid ester according to claim 4, characterized in that: In the step (1), the reaction temperature is 30 to 50° C. and the reaction time is 8 to 24 hours.

6. The method for preparing MXene-modified polyaspartic acid ester according to claim 5, characterized in that: In the step (2), the mass ratio of MXene-NH2 to dialkyl maleate is 10-18:3.5-5.

5.

7. The method for preparing MXene-modified polyaspartic acid ester according to claim 5 or 6, characterized in that: In the step (2), the dropping temperature is 50 to 70° C. and the dropping time is 20 to 50 min; The temperature of the addition reaction is 90-120° C., and the time of the addition reaction is 10-30 minutes.

8. A MXene-modified polyaspartic acid ester prepared by the preparation method of MXene-modified polyaspartic acid ester according to any one of claims 1 to 7.

9. A use of the MXene-modified polyaspartic acid ester according to claim 8 in the preparation of polyurea coatings, characterized in that: The MXene-modified polyaspartic acid ester and the isocyanate curing agent are mixed in butyl acetate to obtain a MXene-modified polyaspartic acid ester polyurea coating; The isocyanate curing agent is a solvent-based isocyanate oligomer.

10. The use of the MXene-modified polyaspartic acid ester in the preparation of polyurea coating according to claim 9, characterized in that: The mass ratio of the MXene-modified polyaspartic acid ester to the isocyanate curing agent is 14-20:5-15; The amount of butyl acetate used is 10 to 50% of the total mass of the MXene-modified polyaspartic acid ester and the isocyanate curing agent.