Preparation method of polyvinyl alcohol film and polyvinyl alcohol film
By modifying mesoporous silica with amino groups and grafting fluoro-containing alkyl chains, and mixing modified polyvinyl alcohol to prepare a water-resistant and ethylene adsorption property, the polyvinyl alcohol film is solved in water The problems of dissolution and poor mechanical strength have achieved the effect of effectively inhibiting ethylene gas and extending the shelf life of food.
Patent Information
- Application Number
- CN202410921318.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-10
- Publication Date
- 2024-11-08
AI Technical Summary
The polyvinyl alcohol film is dissolved in water and has poor mechanical strength, which cannot meet the actual application needs, and cannot effectively inhibit ethylene gas, resulting in accelerated food rot.
By modifying mesoporous silica with amino groups and grafting fluoro-containing alkyl chains through epoxy ring-opening reaction, and blending modified polyvinyl alcohol to prepare a polyvinyl alcohol film that has water resistance and ethylene adsorption properties.
It significantly improves the water resistance and ethylene adsorption properties of the film, can effectively extend the shelf life of food, and meet the needs of food packaging.
Smart Images

Figure CN118909278A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of film preparation, and in particular relates to a preparation method of a polyvinyl alcohol film and the polyvinyl alcohol film. Background Art
[0002] Polyvinyl alcohol has a strict linear polymer structure and stable chemical properties. The hydrogen bonds between molecules form an interlaced lattice structure, which gives it sufficient thermal stability. The large number of hydroxyl groups on the molecular chain makes it highly hydrophilic and has a similar solubility parameter to water, making it a good hydrophilic membrane material. Polyvinyl alcohol has excellent hydrophilic and anti-fouling properties, but it is easy to swell or even dissolve in water, and the mechanical strength of the membrane is poor, which cannot meet the use requirements in practical applications.
[0003] Ethylene is produced as fruits and vegetables mature. Studies have shown that ethylene gas has a ripening effect on fruits and vegetables, and enhances their respiration, playing a decisive role in the maturation and aging of fruits and vegetables. However, polyvinyl alcohol has good oil and chemical solvent resistance, gas barrier properties and biodegradability. Direct use as a food packaging film cannot remove or inhibit ethylene gas, which can easily enhance the respiration intensity of food and accelerate the rate of food decay.
[0004] Ethylene adsorption technology is one of the effective means to remove ethylene or inhibit the action of ethylene. The adsorbent materials used in physical adsorption are mostly gas-adsorbing porous substances, which not only have higher safety and stability than chemical adsorption, but also have special pore structures that have selective permeability to gas adsorption. They can be used as ethylene adsorbents or inorganic fillers to enhance the performance of film substrates.
[0005] CN111995787B discloses a fluorinated PVA / SiO2 super-hydrophobic film and its preparation method. The obtained film is placed in a FAS ethanol solution for fluorination, which solves the problem of poor hydrophobicity of conventional films made of SiO2 and PVA. CN202310871723.8 discloses an ethylene adsorption coating slurry used for fruit and vegetable preservation. The porous material loaded with high-energy potassium acid improves the adsorption efficiency of ethylene and has a significant effect on the preservation of fruits and vegetables. Summary of the invention
[0006] The purpose of this section is to summarize some aspects of embodiments of the present invention and briefly introduce some preferred embodiments. Some simplifications or omissions may be made in this section and the specification abstract and the invention title of this application to avoid blurring the purpose of this section, the specification abstract and the invention title, and such simplifications or omissions cannot be used to limit the scope of the present invention.
[0007] In view of the above problems and / or the problems existing in the prior art, the present invention is proposed.
[0008] Therefore, the object of the present invention is to overcome the deficiencies in the prior art and provide a method for preparing a polyvinyl alcohol film.
[0009] In order to solve the above technical problems, the present invention provides the following technical solutions: a method for preparing a polyvinyl alcohol film, comprising:
[0010] Modifying mesoporous silica with amino groups to obtain amino-modified mesoporous silica;
[0011] The amino-modified mesoporous silica was subjected to epoxy ring-opening reaction and grafted with fluorinated alkyl chains to obtain modified mesoporous silica;
[0012] The modified mesoporous silica was mixed with modified polyvinyl alcohol to prepare a water-resistant polyvinyl alcohol film with ethylene adsorption performance.
[0013] As a preferred embodiment of the preparation method of the present invention, the mesoporous silica is modified by amino groups, and the modification method includes:
[0014] Take mesoporous silica and add solvent, add amino modifier after heating, condense and reflux, cool and centrifuge;
[0015] The product was washed with deionized water and anhydrous ethanol for multiple times and dried in vacuum to obtain amino-modified mesoporous silica.
[0016] As a preferred embodiment of the preparation method of the present invention, the solvent comprises anhydrous toluene.
[0017] As a preferred embodiment of the preparation method of the present invention, the amino modifier includes one of γ-aminopropyltriethoxysilane, γ-aminopropyltrimethoxysilane, N-β (aminopropyl)-γ-aminopropylmethyldimethoxysilane, N-β (aminopropyl)-γ-aminopropyltrimethoxysilane, N-β (aminopropyl)-γ-aminopropylmethyltriethoxysilane, and N-β (aminopropyl)-γ-aminopropyltriethoxysilane.
[0018] As a preferred embodiment of the preparation method of the present invention, wherein: the amino-modified mesoporous silica is subjected to an epoxy ring-opening reaction, comprising:
[0019] adding a fluorinated alkyl chain to a solvent to obtain a fluorinated alkyl chain solution;
[0020] adding amino-modified mesoporous silica into a solvent to obtain an amino-modified mesoporous silica suspension;
[0021] The fluorinated alkyl chain solution and the amino-modified mesoporous silica suspension are mixed, and the temperature is raised to 80-90° C. under a nitrogen atmosphere to react for 3-5 hours. The obtained product is filtered, washed with ethanol for multiple times, and vacuum dried to obtain modified mesoporous silica.
[0022] As a preferred embodiment of the preparation method of the present invention, the fluorinated alkyl chain is one of perfluorooctyl propylene oxide, perfluorohexyl propylene oxide, perfluorobutyl propylene oxide and perfluoropropylene oxide.
[0023] As a preferred embodiment of the preparation method of the present invention, wherein: the fluorinated alkyl chain is added to the solvent, wherein the solvent includes N,N-dimethylformamide, and the ratio of the fluorinated alkyl chain to the solvent is 0.2-1 g:30-50 mL; the amino-modified mesoporous silica is added to the solvent, wherein the solvent includes N,N-dimethylformamide, and the ratio of the amino-modified mesoporous silica to the solvent is 1-2 g:20-40 mL.
[0024] As a preferred embodiment of the preparation method of the present invention, the fluorinated alkyl chain solution and the amino-modified mesoporous silica suspension are mixed, wherein the ratio of the fluorinated alkyl chain solution to the amino-modified mesoporous silica suspension is 20-30 mL:20-40 mL.
[0025] As a preferred embodiment of the preparation method of the present invention, the preparation of the water-resistant polyvinyl alcohol film having ethylene adsorption performance comprises:
[0026] Modified mesoporous silica is mixed with modified polyvinyl alcohol, reacted for 2-4 hours, glycerol is added, reacted for 20-60 minutes, vacuum degassing is performed, the coating liquid is poured on a coating machine, a film is scraped, and the film is peeled off after heating and drying to obtain a thin film;
[0027] The mass ratio of the modified mesoporous silica to the modified polyvinyl alcohol is 2-4%.
[0028] Another object of the present invention is to overcome the deficiencies in the prior art and provide a method for preparing a polyvinyl alcohol film which is water-resistant and has the ability to absorb ethylene.
[0029] Beneficial effects of the present invention:
[0030] (1) The present invention greatly improves the poor water resistance and ethylene adsorption performance of the polyvinyl alcohol film by introducing modified mesoporous silica. The mesoporous silica itself is a good adsorbent material, and its high specific surface area and special pore structure provide ethylene gas adsorption sites. The fluorinated alkyl chain is grafted by epoxy ring-opening reaction, and the low surface energy of the fluorinated substance is beneficial to enhancing the water resistance of the surface of the polyvinyl alcohol film.
[0031] (2) The reaction conditions of the present invention are mild, and the modified polyvinyl alcohol film can be used as a good food packaging material, which can meet the actual packaging needs while reducing the ethylene gas that promotes ripening and aging, and effectively extend the shelf life of food. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the following briefly introduces the drawings required for describing the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative labor. Among them:
[0033] Figure 1 This is a test diagram of the hydrophobicity of the film before and after modification in the embodiment of the present invention. DETAILED DESCRIPTION
[0034] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are described in detail below in conjunction with the embodiments of the specification.
[0035] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention may also be implemented in other ways different from those described herein, and those skilled in the art may make similar generalizations without violating the connotation of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed below.
[0036] Secondly, the term "one embodiment" or "embodiment" as used herein refers to a specific feature, structure, or characteristic that may be included in at least one implementation of the present invention. The term "in one embodiment" that appears in different places in this specification does not necessarily refer to the same embodiment, nor does it refer to a separate or selective embodiment that is mutually exclusive with other embodiments.
[0037] The amino modifier in the present invention is one of γ-aminopropyltriethoxysilane, γ-aminopropyltrimethoxysilane, N-β (aminopropyl)-γ-aminopropylmethyldimethoxysilane, N-β (aminopropyl)-γ-aminopropyltrimethoxysilane, N-β (aminopropyl)-γ-aminopropylmethyltriethoxysilane, and N-β (aminopropyl)-γ-aminopropyltriethoxysilane, all of which are common commercial products;
[0038] The fluorinated alkyl chain is one of perfluorooctyl propylene oxide, perfluorohexyl propylene oxide, perfluorobutyl propylene oxide, and perfluoropropylene oxide, all of which are common commercial products;
[0039] The polyvinyl alcohol is one of 0588, 0788, 2488, 1799, 1788, Kuraray 217 and 117, all of which are common commercially available products.
[0040] The mesoporous silica in the embodiment of the present invention has a particle size of 3 μm and was purchased from Hefei Qianguo New Material Technology Co., Ltd.
[0041] Film testing method in the embodiment of the present invention:
[0042] Mechanical properties: The tensile strength of the film is determined using the national standard GB / T 1040.3-2006 Test conditions for tensile properties of plastics Part 3 Thin plastics and sheets;
[0043] Water resistance: The contact angle of the film was measured using a contact angle meter;
[0044] Ethylene elimination performance: After the film is made into a sealed fresh-keeping bag, 1 mL of ethylene gas is injected into the fresh-keeping bag with a syringe. After 24 hours, the reduced value of ethylene gas concentration in the fresh-keeping packaging bag is measured by gas chromatograph.
[0045] Example 1
[0046] (1) Weigh 1 g of mesoporous silica, add 30 mL of anhydrous toluene, heat to 90 °C, add 1.5 mL of amino modifier (γ-aminopropyltriethoxysilane, i.e. KH550), condense and reflux for 12 h, cool and centrifuge, wash with deionized water and anhydrous ethanol several times, and dry in vacuum at 40 °C. The obtained product is MS@NH2.
[0047] (2) Take 0.2 g of fluorinated alkyl chain (perfluoropropylene oxide), add 30 mL of N,N-dimethylformamide (DMF), and stir to dissolve at 60°C;
[0048] Take another 1gMS@NH2, pour into 25mL DMF, and stir and disperse at 40℃ for 10min;
[0049] The completely dissolved fluorinated alkyl chain solution was poured into the MS@NH2 suspension and heated to 80°C for 5 h under a nitrogen atmosphere. The obtained product was filtered, washed with ethanol several times, and dried in a vacuum oven at 40°C overnight to obtain MS-F;
[0050] (3) Add polyvinyl alcohol (1799) to deionized water to prepare an 8% solution, and heat to 90°C for 2 h;
[0051] Ultrasonic dispersion of 2% mass fraction of polyvinyl alcohol MS-F in polyvinyl alcohol mother liquor, react for 2 hours, add 0.4g glycerol, react for 30 minutes, vacuum degassing, pour the above coating liquid on a coating machine, scrape the film, heat and dry at 40°C, and then peel off the film to obtain a PVA / MS-F film.
[0052] The hydrophobicity test diagram of the film before and after modification in this embodiment is shown in Figure 1 .
[0053] Example 2
[0054] (1) Weigh 1 g of mesoporous silica, add 30 mL of anhydrous toluene, heat to 90 °C, add 1.5 mL of amino modifier (γ-aminopropyltriethoxysilane, i.e. KH550), condense and reflux for 12 h, cool and centrifuge, wash with deionized water and anhydrous ethanol several times, and dry in vacuum at 40 °C. The obtained product is MS@NH2.
[0055] (2) Take 0.2 g of fluorinated alkyl chain (perfluorobutyl propylene oxide), add 30 mL of N, N-dimethylformamide (DMF), and stir to dissolve at 60 °C;
[0056] Take another 1gMS@NH2, pour into 25mL DMF, and stir and disperse at 40℃ for 10min;
[0057] The completely dissolved fluorinated alkyl chain solution was poured into the MS@NH2 suspension and heated to 80°C for 5 h under a nitrogen atmosphere. The obtained product was filtered, washed with ethanol several times, and dried in a vacuum oven at 40°C overnight to obtain MS-F;
[0058] (3) Add polyvinyl alcohol (1799) to deionized water to prepare an 8% solution, and heat to 90°C for 2 h;
[0059] Ultrasonic dispersion of 2% mass fraction of polyvinyl alcohol MS-F in polyvinyl alcohol mother liquor, react for 2 hours, add 0.4g glycerol, react for 30 minutes, vacuum degassing, pour the above coating liquid on a coating machine, scrape the film, heat and dry at 40°C, and then peel off the film to obtain a PVA / MS-F film.
[0060] Example 3
[0061] (1) Weigh 1 g of mesoporous silica, add 30 mL of anhydrous toluene, heat to 90 °C, add 1.5 mL of amino modifier (γ-aminopropyltriethoxysilane, i.e. KH550), condense and reflux for 12 h, cool and centrifuge, wash with deionized water and anhydrous ethanol several times, and dry in vacuum at 40 °C. The obtained product is MS@NH2.
[0062] (2) Take 0.2 g of fluorinated alkyl chain (perfluorohexyl propylene oxide), add 30 mL of N,N-dimethylformamide (DMF), and stir to dissolve at 60°C;
[0063] Take another 1gMS@NH2, pour into 25mL DMF, and stir and disperse at 40℃ for 10min;
[0064] The completely dissolved fluorinated alkyl chain solution was poured into the MS@NH2 suspension and heated to 80°C for 5 h under a nitrogen atmosphere. The obtained product was filtered, washed with ethanol several times, and dried in a vacuum oven at 40°C overnight to obtain MS-F;
[0065] (3) Add polyvinyl alcohol (1799) to deionized water to prepare an 8% solution, and heat to 90°C for 2 h;
[0066] Ultrasonic dispersion of 2% mass fraction of polyvinyl alcohol MS-F in polyvinyl alcohol mother liquor, react for 2 hours, add 0.4g glycerol, react for 30 minutes, vacuum degassing, pour the above coating liquid on a coating machine, scrape the film, heat and dry at 40°C, and then peel off the film to obtain a PVA / MS-F film.
[0067] Example 4
[0068] (1) Weigh 1 g of mesoporous silica, add 30 mL of anhydrous toluene, heat to 90 °C, add 1.5 mL of amino modifier (γ-aminopropyltriethoxysilane, i.e. KH550), condense and reflux for 12 h, cool and centrifuge, wash with deionized water and anhydrous ethanol several times, and dry in vacuum at 40 °C. The obtained product is MS@NH2.
[0069] (2) Take 0.2 g of fluorinated alkyl chain (perfluorooctyl propylene oxide), add 30 mL of N,N-dimethylformamide (DMF), and stir to dissolve at 60°C;
[0070] Take another 1gMS@NH2, pour into 25mL DMF, and stir and disperse at 40℃ for 10min;
[0071] The completely dissolved fluorinated alkyl chain solution was poured into the MS@NH2 suspension and heated to 80°C for 5 h under a nitrogen atmosphere. The obtained product was filtered, washed with ethanol several times, and dried in a vacuum oven at 40°C overnight to obtain MS-F;
[0072] (3) Add polyvinyl alcohol (1799) to deionized water to prepare an 8% solution, and heat to 90°C for 2 h;
[0073] Ultrasonic dispersion of 2% mass fraction of polyvinyl alcohol MS-F in polyvinyl alcohol mother liquor, react for 2 hours, add 0.4g glycerol, react for 30 minutes, vacuum degassing, pour the above coating liquid on a coating machine, scrape the film, heat and dry at 40°C, and then peel off the film to obtain a PVA / MS-F film.
[0074] Comparative Example 1
[0075] Preparation method of pure PVA:
[0076] Add polyvinyl alcohol into deionized water to prepare a solution with a concentration of 8%, heat to 90°C and mechanically stir to react for 2 hours, vacuum degassing, pour the coating solution onto a coating machine and scrape the film, heat to 40°C and dry, then peel off the film.
[0077] Comparative Example 2
[0078] The preparation method of this comparative example is the same as that of Example 1, except that the mesoporous silica is changed to solid, and the other conditions are the same as those of Example 1.
[0079] Comparative Example 3
[0080] The mesoporous silica was not amino-modified, and other conditions were the same as those in Example 1:
[0081] (1) Take 0.2 g of fluorinated alkyl chain (perfluoropropylene oxide), add 30 mL of N,N-dimethylformamide (DMF), and stir to dissolve at 60°C;
[0082] Take another 1g of mesoporous silica, pour into 25mL of DMF, and stir and disperse at 40°C for 10min to prepare a suspension;
[0083] The completely dissolved fluorinated alkyl chain solution was poured into the suspension, and the temperature was raised to 80°C for reaction for 5 h under nitrogen atmosphere. The obtained product was filtered, washed with ethanol several times, and dried in a vacuum oven at 40°C overnight to obtain MS-F;
[0084] (2) Add polyvinyl alcohol (1799) to deionized water to prepare an 8% solution, and heat to 90°C for 2 h;
[0085] 2% mass fraction of polyvinyl alcohol MS-F was ultrasonically dispersed in polyvinyl alcohol mother liquor, reacted for 2 h, 0.4 g of glycerol was added, reacted for 30 min, and vacuum degassing was performed;
[0086] The coating liquid was poured onto a coating machine and scraped, and then heated and dried at 40°C and peeled off to obtain a PVA / MS-F film.
[0087] Comparative Example 4
[0088] Under the conditions of Example 1, no epoxy ring-opening reaction was performed, and other conditions were the same as those of Example 1:
[0089] (1) Weigh 1 g of mesoporous silica, add 30 mL of anhydrous toluene, heat to 90 °C, add 1.5 mL of amino modifier (γ-aminopropyltriethoxysilane, i.e. KH550), condense and reflux for 12 h, cool and centrifuge, wash with deionized water and anhydrous ethanol several times, and dry in vacuum at 40 °C. The obtained product is MS@NH2.
[0090] (2) Add polyvinyl alcohol (1799) to deionized water to prepare an 8% solution, and heat to 90°C for 2 h;
[0091] 2% mass fraction of polyvinyl alcohol MS@NH2 was ultrasonically dispersed in polyvinyl alcohol mother liquor, reacted for 2 h, 0.4 g glycerol was added, reacted for 30 min, and vacuum degassing was performed;
[0092] The coating liquid was poured onto a coating machine and scraped, and the film was removed after heating and drying at 40°C to obtain a PVA / MS film.
[0093] Comparative Example 5
[0094] Under the conditions of Example 1, the epoxy ring-opening reaction conditions were improperly controlled, and the other conditions were the same as in Example 1:
[0095] (1) Weigh 1 g of mesoporous silica, add 30 mL of anhydrous toluene, heat to 90 °C, add 1.5 mL of amino modifier (γ-aminopropyltriethoxysilane, i.e. KH550), condense and reflux for 12 h, cool and centrifuge, wash with deionized water and anhydrous ethanol several times, and dry in vacuum at 40 °C. The obtained product is MS@NH2.
[0096] (2) Take 0.2 g of fluorinated alkyl chain (perfluoropropylene oxide), add 30 mL of N,N-dimethylformamide (DMF), and stir to dissolve at 60°C;
[0097] Take another 1gMS@NH2, pour into 25mL DMF, and stir and disperse at 40℃ for 10min;
[0098] The completely dissolved fluorinated alkyl chain solution was poured into the MS@NH2 suspension and heated to 60°C for 5 h under a nitrogen atmosphere. The obtained product was filtered, washed with ethanol several times, and dried in a vacuum oven at 40°C overnight to obtain MS-F;
[0099] (3) Add polyvinyl alcohol (1799) to deionized water to prepare an 8% solution, and heat to 90°C for 2 h;
[0100] Ultrasonic dispersion of 2% mass fraction of polyvinyl alcohol MS-F in polyvinyl alcohol mother liquor, react for 2 hours, add 0.4g glycerol, react for 30 minutes, vacuum degassing, pour the above coating liquid on a coating machine, scrape the film, heat and dry at 40°C, and then peel off the film to obtain a PVA / MS-F film.
[0101] Comparative Example 6
[0102] Under the conditions of Example 1, the amount of modified mesoporous silica blended with modified polyvinyl alcohol is inappropriate:
[0103] (1) Weigh 1 g of mesoporous silica, add 30 mL of anhydrous toluene, heat to 90 °C, add 1.5 mL of amino modifier (γ-aminopropyltriethoxysilane, i.e. KH550), condense and reflux for 12 h, cool and centrifuge, wash with deionized water and anhydrous ethanol several times, and dry in vacuum at 40 °C. The obtained product is MS@NH2.
[0104] (2) Take 0.2 g of fluorinated alkyl chain (perfluoropropylene oxide), add 30 mL of N,N-dimethylformamide (DMF), and stir to dissolve at 60°C;
[0105] Take another 1gMS@NH2, pour into 25mL DMF, and stir and disperse at 40℃ for 10min;
[0106] The completely dissolved fluorinated alkyl chain solution was poured into the MS@NH2 suspension and heated to 80°C for 5 h under a nitrogen atmosphere. The obtained product was filtered, washed with ethanol several times, and dried in a vacuum oven at 40°C overnight to obtain MS-F;
[0107] (3) Add polyvinyl alcohol (1799) to deionized water to prepare an 8% solution, and heat to 90°C for 2 h;
[0108] 1% mass fraction of polyvinyl alcohol MS-F was ultrasonically dispersed in the polyvinyl alcohol mother liquor, reacted for 2 hours, 0.4g of glycerol was added, reacted for 30 minutes, and vacuum degassing was performed. The above coating liquid was poured on a coating machine and the film was scraped. After heating and drying at 40°C, the film was peeled off to obtain a PVA / MS-F film.
[0109] Comparative Example 7
[0110] (1) Weigh 1 g of mesoporous silica, add 30 mL of anhydrous toluene, heat to 90 °C, add 1.5 mL of amino modifier (γ-aminopropyltriethoxysilane, i.e. KH550), condense and reflux for 12 h, cool and centrifuge, wash with deionized water and anhydrous ethanol several times, and dry in vacuum at 40 °C. The obtained product is MS@NH2.
[0111] (2) Take 0.2 g of fluorinated alkyl chain (perfluoropropylene oxide), add 30 mL of N,N-dimethylformamide (DMF), and stir to dissolve at 60°C;
[0112] Take another 1gMS@NH2, pour into 25mL DMF, and stir and disperse at 40℃ for 10min;
[0113] The completely dissolved fluorinated alkyl chain solution was poured into the MS@NH2 suspension and heated to 80°C for 5 h under a nitrogen atmosphere. The obtained product was filtered, washed with ethanol several times, and dried in a vacuum oven at 40°C overnight to obtain MS-F;
[0114] (3) Add polyvinyl alcohol (1799) to deionized water to prepare an 8% solution, and heat to 90°C for 2 h;
[0115] 4% mass fraction of polyvinyl alcohol MS-F was ultrasonically dispersed in polyvinyl alcohol mother liquor, reacted for 2h, 0.4g glycerol was added, reacted for 30min, vacuum degassing was carried out, the above coating liquid was poured on a coating machine and the film was scraped, heated and dried at 40℃ and then peeled off to obtain PVA / MS-F film.
[0116] Comparative Example 8
[0117] (1) Weigh 1 g of mesoporous silica, add 30 mL of anhydrous toluene, heat to 90 °C, add 1.5 mL of amino modifier (γ-aminopropyltriethoxysilane, i.e. KH550), condense and reflux for 12 h, cool and centrifuge, wash with deionized water and anhydrous ethanol several times, and dry in vacuum at 40 °C. The obtained product is MS@NH2.
[0118] (2) Add polyvinyl alcohol (1799) to deionized water to prepare an 8% solution, and heat to 90°C for 2 h;
[0119] 2% mass fraction of polyvinyl alcohol MS@NH2 was ultrasonically dispersed in polyvinyl alcohol mother liquor, reacted for 2 h, 0.4 g glycerol was added, reacted for 30 min, and vacuum degassing was performed;
[0120] The coating liquid is poured onto a coating machine and scraped, and then heated and dried at 40°C and peeled off to obtain a PVA / MS film;
[0121] (3) Take 0.2 g of fluorinated alkyl chain (perfluoropropylene oxide), add 30 mL of N,N-dimethylformamide (DMF), and stir to dissolve at 60°C;
[0122] The obtained PVA / MS film was immersed in a DMF solution of perfluoropropylene oxide for 2 h, and its performance was measured after drying.
[0123] The experimental results are shown in Table 1.
[0124] Table 1
[0125] Mechanical strength / MPa Contact angle / ° Ethylene elimination rate / % Example 1 (perfluoropropylene oxide) 39.26 84.32 83.1 Example 2 (perfluorobutyl propylene oxide) 38.05 83.74 84.2 Example 3 (perfluorohexyl propylene oxide) 34.23 85.63 82.4 Example 4 (Perfluorooctylpropylene oxide) 31.68 88.14 78.6 Comparative Example 1 (pure PVA) 34.34 47.13 13.5 Comparative Example 2 (Silicon dioxide is non-porous) 38.61 80.64 50.2 Comparative Example 3 (PVA / MS / F) 35.35 65.21 81.4 Comparative Example 4 (PVA / MS) 36.17 50.47 84.6 Comparative Example 5 35.64 52.64 83.7 Comparative Example 6 35.33 75.39 67.3 Comparative Example 7 42.24 80.45 86.2 Comparative Example 8 34.82 73.64 77.53
[0126] As can be seen from Table 1, the water resistance and ethylene elimination ability of pure PVA in Comparative Example 1 are relatively weak; after adding an appropriate amount of mesoporous silica to graft fluorinated alkyl chains in the embodiment, the performance of the film is significantly improved, and the fluorinated substance with low surface energy improves the water resistance of the film. Silica not only increases the surface roughness of the film, but also the mesoporous silica provides a large number of adsorption sites for the elimination of ethylene; after adding non-porous silica to Comparative Example 2, the contact angle of the film is significantly improved, and the water resistance is improved, but the sites for ethylene adsorption on the surface are less, and the ethylene elimination ability is relatively weak; Comparative Example 3 is not grafted with fluorinated alkyl chains by epoxy ring-opening reaction, but the addition of silica makes the surface of the film rough, the water resistance is improved, the contact angle is increased, and the ethylene elimination rate is higher; Comparative Example 4 is similar to Comparative Example 3;
[0127] In comparative example 5, the temperature of the ring-opening reaction was relatively low, which affected the grafting rate of the fluorinated alkyl chain and resulted in poor water resistance of the film;
[0128] In Comparative Example 6, insufficient addition of silica limited the adsorption capacity of silica, and the ethylene elimination rate was not significantly improved; in Comparative Example 7, excessive silica was prone to agglomeration, and no longer adsorbed ethylene after reaching saturation;
[0129] In Comparative Example 8, the fluorine-containing substance is enriched on the membrane surface by immersion. This interaction is weaker than the grafting effect of the ring-opening reaction. Although the water resistance of the film is improved, the contact angle is smaller than the chemical grafting of fluorine-containing alkyl chains.
[0130] It should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solutions of the present invention can be modified or replaced by equivalents without departing from the spirit and scope of the technical solutions of the present invention, which should all be included in the scope of the present invention.
Claims
1. A method for preparing a polyvinyl alcohol film, characterized in that: include, Modifying mesoporous silica with amino groups to obtain amino-modified mesoporous silica; The amino-modified mesoporous silica was subjected to epoxy ring-opening reaction and grafted with fluorinated alkyl chains to obtain modified mesoporous silica; The modified mesoporous silica was mixed with modified polyvinyl alcohol to prepare a water-resistant polyvinyl alcohol film with ethylene adsorption performance.
2. The preparation method according to claim 1, characterized in that: The mesoporous silica is modified by amino groups, and the modification method includes: Take mesoporous silica and add solvent, add amino modifier after heating, condense and reflux, cool and centrifuge; The product was washed with deionized water and anhydrous ethanol for multiple times and dried in vacuum to obtain amino-modified mesoporous silica.
3. The preparation method according to claim 2, characterized in that: The solvent includes anhydrous toluene.
4. The preparation method according to claim 2 or 3, characterized in that: The amino modifier includes one of γ-aminopropyltriethoxysilane, γ-aminopropyltrimethoxysilane, N-β (aminopropyl)-γ-aminopropylmethyldimethoxysilane, N-β (aminopropyl)-γ-aminopropyltrimethoxysilane, N-β (aminopropyl)-γ-aminopropylmethyltriethoxysilane, and N-β (aminopropyl)-γ-aminopropyltriethoxysilane.
5. The preparation method according to claim 1, characterized in that: The amino-modified mesoporous silica is subjected to an epoxy ring-opening reaction, comprising: adding a fluorinated alkyl chain to a solvent to obtain a fluorinated alkyl chain solution; adding amino-modified mesoporous silica into a solvent to obtain an amino-modified mesoporous silica suspension; The fluorinated alkyl chain solution and the amino-modified mesoporous silica suspension are mixed, and the temperature is raised to 80-90° C. under a nitrogen atmosphere to react for 3-5 hours. The obtained product is filtered, washed with ethanol for multiple times, and vacuum dried to obtain modified mesoporous silica.
6. The preparation method according to claim 5, characterized in that: The fluorine-containing alkyl chain is one of perfluorooctyl propylene oxide, perfluorohexyl propylene oxide, perfluorobutyl propylene oxide and perfluoropropylene oxide.
7. The preparation method according to claim 5, characterized in that: The fluorinated alkyl chain is added to the solvent, wherein the solvent includes N,N-dimethylformyl, and the ratio of the fluorinated alkyl chain to the solvent is 0.2-1 g:30-50 mL; the amino-modified mesoporous silica is added to the solvent, wherein the solvent includes N,N-dimethylformyl, and the ratio of the amino-modified mesoporous silica to the solvent is 1-2 g:20-40 mL.
8. The preparation method according to claim 5, characterized in that: The fluorinated alkyl chain solution and the amino-modified mesoporous silica suspension are mixed, wherein the ratio of the fluorinated alkyl chain solution to the amino-modified mesoporous silica suspension is 20-30 mL:20-40 mL.
9. The preparation method according to claim 1, characterized in that: The polyvinyl alcohol film prepared in the above method is water-resistant and has the ability to absorb ethylene. include, Modified mesoporous silica is mixed with modified polyvinyl alcohol, reacted for 2-4 hours, glycerol is added, reacted for 20-60 minutes, vacuum degassing is performed, the coating liquid is poured on a coating machine, a film is scraped, and the film is peeled off after heating and drying to obtain a thin film; The mass ratio of the modified mesoporous silica to the modified polyvinyl alcohol is 2-4%.
10. The water-resistant polyvinyl alcohol film having ethylene adsorption performance obtained by the preparation method according to any one of claims 1 to 9.
Citation Information
Patent Citations
Fluorinated PVA / SiO2 superhydrophobic film and its preparation method
CN111995787B
Ethylene adsorption coating slurry applied to fresh keeping of fruits and vegetables as well as preparation method and application of ethylene adsorption coating slurry
CN116948464A
Cited By
High-adsorption cooling film for grape planting and preparation method thereof
CN119974716A
A high-adsorption cooling film for grape cultivation and preparation method thereof
CN119974716B