Preparation method of large-size open-cell negative poisson ratio foam material

Through the three-axis-by-axis compression, heating and cooling methods, the problem of uneven performance of large-size open-pore negative Poisson's foam material is solved, and the performance uniformity of foam material is significantly improved, satisfying the content of large-size foam materials. Requirements in applications.

CN118909304APending Publication Date: 2024-11-08SHAANXI COAL & CHEM TECH INST +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411151214.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The prior art is difficult to effectively prepare large-size open-pore negative Poisson ratio foam materials, resulting in uneven product performance and unable to meet application needs.

Method used

Three-axis-by-axis compression, heating and cooling are used to overcompress and return to the specified compression position along the X-axis, Y-axis, and Z-axis directions. The overcompression ratio is between 10% and 40%, and the compression at the specified compression position is The ratio is between 50% and 85% to improve the performance uniformity of foam materials.

Benefits of technology

The performance uniformity of large-size open-pore negative Poisson's ratio foam material is significantly improved, ensuring that the Poisson's ratio and density difference of the foam material is within the appropriate range, and improving the overall performance stability of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_2
    Figure FT_2
  • Figure FT_3
    Figure FT_3
Patent Text Reader

Abstract

The invention discloses a preparation method of a large-size open-cell negative poisson ratio foam material, and belongs to the technical field of foam materials. The preparation method of the large-size open-cell negative Poisson's ratio foam comprises the following steps: carrying out three-axis-by-axis compression, heating and cooling on open-cell foam to obtain the large-size open-cell negative Poisson's ratio foam, the three-axis-by-axis compression comprises the steps of performing excess compression in the X-axis direction, the Y-axis direction and the Z-axis direction and returning to the specified compression amount position; the ratio of excess compression is independently selected from 10%-40%; the compression ratio of the specified compression amount position is independently selected from 50%-85%. According to the preparation method, the large-size open-cell negative Poisson's ratio foam material of which the performance uniformity is remarkably improved is prepared by performing three-axis-by-axis excess compression on open-cell foam and returning the open-cell foam to a specified compression amount position for the first time.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of foam materials, and in particular to a method for preparing a large-size open-cell negative Poisson's ratio foam material. Background Art

[0002] Auxetic foams, also known as negative Poisson's ratio foams, expand laterally when stretched and contract laterally when compressed, exhibiting negative Poisson's ratio behavior. Poisson's ratio is an elastic property of a material that describes the deformation behavior of a material when subjected to stress, where a positive Poisson's ratio means that the material becomes thinner when stretched, while a negative Poisson's ratio means that the material expands when stretched. The behavior of negative Poisson's ratio materials under specific stress conditions is generally less common, but they are valuable in some special applications, such as thermal insulation and shock absorption.

[0003] The negative Poisson's ratio foam material has a concave corner, folded or rotated cell structure. Its unique tensile expansion behavior makes it have the characteristics of light weight, heat insulation and noise reduction of general polymer foam, as well as good indentation resistance, strong fracture toughness and good notch resistance. In particular, it shows excellent buffering and energy absorption characteristics in dynamic impact tests. Therefore, the negative Poisson's ratio foam material has broad application prospects in many fields such as sports protection buffer materials, shockproof gloves, advanced cushions and mattresses, sandwich panels, sensors, controllable filter materials, seat belts, bumpers, artificial blood vessels, etc.

[0004] Since Professor Lakes first prepared open-cell polyurethane auxetic foam in 1978, open-cell auxetic foam (also known as open-cell negative Poisson's ratio foam) has received extensive attention and research. The preparation methods of open-cell auxetic foam usually include triaxial hot compression, biaxial compression, multiphase triaxial hot compression, chemical mechanical process and semi-mold manufacturing. However, these methods are basically still at the level of preparing small-sized foam in the laboratory. Florida State University applied for invention patent CN201580041085 in 2015, and produced it with Auxadyne Company in the United States, launching the first PU open-cell auxetic foam product - Xylafoam, and it has been successfully applied to products such as prosthetic sheaths, corrective insoles and cushions, ankle support protection systems, football helmets, ski helmets, and saddle cushions.

[0005] With the application of open-cell negative Poisson's ratio foam materials, people have an urgent need for the preparation technology of large-sized negative Poisson's ratio open-cell foams and improving the uniformity of large-sized negative Poisson's ratio open-cell foams.

[0006] In order to achieve compression of large-volume open-cell negative Poisson's ratio foam materials, a three-axis compression method can be used, that is, the equipment only performs compression movement in one axial direction each time, and after completing the compression of one axial direction, it compresses the other axial direction one by one, thereby finally completing the three-axis compression. However, this sequential compression process easily causes the compression degree of the foam close to the moving push plate to be much higher than the compression degree of the foam far away from the moving push plate, thereby causing the problem of uneven product performance.

[0007] Therefore, research and development of a new preparation method for large-size open-cell negative Poisson's ratio foam materials is of great significance for the application of open-cell negative Poisson's ratio foams. Summary of the invention

[0008] In view of this, the technical problem to be solved by the present invention is to provide a method for preparing a large-sized open-cell negative Poisson's ratio foam material. The preparation method significantly improves the performance uniformity of the large-sized open-cell negative Poisson's ratio foam material.

[0009] In order to achieve the above purpose, the technical solution adopted by the present invention is as follows:

[0010] The present invention provides a method for preparing a large-size open-cell negative Poisson's ratio foam, comprising the following steps:

[0011] The open-cell foam is subjected to triaxial compression, heating, and cooling to obtain a large-size open-cell negative Poisson's ratio foam;

[0012] The three-axis compression is to perform over-compression and return to the specified compression amount position along the X-axis, Y-axis and Z-axis directions respectively;

[0013] Preferably, the excess compression ratio is independently selected from 10% to 40%; more preferably, the excess compression ratio is independently selected from 20% to 40%. In some specific embodiments of the present invention, it is preferably 20%, 30% or 40%.

[0014] Preferably, the compression ratio of the designated compression position is independently selected from 50% to 85%; more preferably, the compression ratio of the designated compression position is independently selected from 58% to 85%. In some specific embodiments of the present invention, it is preferably 58%, 60%, 69%, or 85%.

[0015] The present invention significantly improves the performance uniformity of the prepared open-cell negative Poisson's ratio foam by over-compressing and returning to a specified compression position.

[0016] The performance uniformity or performance uniformity described in the present invention refers to the property of "Poisson's ratio".

[0017] Preferably, the open-cell foam is selected from polyurethane foam, melamine foam or polyimide foam.

[0018] Preferably, the heating temperature is 160 o C~260 o C;

[0019] Preferably, the heating time is 1 to 12 h.

[0020] The present invention does not specifically limit the heating method, and it can be a heating method well known to those skilled in the art.

[0021] The heating methods include but are not limited to oven heating, hot steam heating, etc.

[0022] Preferably, the cooling is cooling to 0 o C~30 o C.

[0023] Preferably, the open-cell foam is in the shape of a cuboid, and the lengths of the three sides are independently selected from 0.2 to 2.5 m.

[0024] Preferably, in the present invention, the length ratio of the longest side to the shortest side of the open-cell foam is ≤3; more preferably, the length ratio of the longest side to the shortest side of the open-cell foam is ≤2.

[0025] The present invention also provides a large-size open-cell negative Poisson's ratio foam material, which is prepared by the above-mentioned preparation method.

[0026] Preferably, in the present invention, the absolute value of the difference in initial Poisson's ratio between the skin layer and the core layer of the large-size open-cell negative Poisson's ratio foam material after stretching is ≤0.2.

[0027] Preferably, the density difference of the large-size open-cell negative Poisson's ratio foam material is ≤30%.

[0028] Preferably, the three-side dimensions of the large-size open-cell negative Poisson's ratio foam material are independently selected from 0.1 to 2.125 m.

[0029] The three dimensions are length, width and height, and the three dimensions can be the same or different.

[0030] Compared with the prior art, the preparation method of the large-sized open-cell negative Poisson's ratio foam provided by the present invention comprises the following steps: subjecting the open-cell foam to triaxial compression, heating and cooling to obtain the large-sized open-cell negative Poisson's ratio foam; the triaxial compression is respectively over-compression along the X-axis, Y-axis and Z-axis directions and retraction to the specified compression amount position; the over-compression ratio is independently selected from 10% to 40%; the compression ratio at the specified compression amount position is independently selected from 50% to 85%. The preparation method is the first to prepare a large-sized open-cell negative Poisson's ratio foam material with significantly improved performance uniformity by over-compressing the open-cell foam triaxially and retracting it to the specified compression amount position. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 A schematic diagram of a triaxial compression device used in the present invention;

[0032] Figure 2 This is a photo of the fixed mold of the triaxial compression device of the present invention;

[0033] Figure 3 This is a photo of the movable mold of the triaxial compression device of the present invention;

[0034] Figure 4 Scanning electron microscope photograph of the polyurethane negative Poisson's ratio foam prepared in Example 1. DETAILED DESCRIPTION

[0035] In order to further illustrate the present invention, the method for preparing the large-size open-cell negative Poisson's ratio foam provided by the present invention is described in detail below in conjunction with examples.

[0036] The over-compression refers to continuing the compression after the compression reaches a specified thickness.

[0037] Excess compression ratio = (specified thickness after compression - thickness of foam at excess compression) / original thickness of foam.

[0038] Compression ratio = specified thickness after compression / original thickness of foam.

[0039] Figure 1 Schematic diagram of the triaxial compression apparatus used in the present invention.

[0040] The three-axis compression equipment is composed of an operating system and an electric control system;

[0041] The operating system includes an equipment support and a fixed mold, a movable mold, four electric screw push rods, and four push plates on the equipment support;

[0042] Among them, the X-axis, Y-axis, Z-axis and the negative Z-axis mold surface of the fixed mold are all provided with notches, and the notches are respectively formed by the X-plate, Y-plate, Z-plate of the four push plates. 1 Plate, Z2 Plate filling, the mold surface and four push plates together form a hollow internal space for filling the compressed object;

[0043] There is a gap of 1 to 5 mm around the four push plates and between the mold surface to prevent hard friction during movement.

[0044] The X plate is located at the upper opening of the fixed mold, and the Y plate is located at the lower end of the opening in front of the fixed mold, wherein the length of the X plate in the Y-axis direction is 99% to 100% of the length of the fixed mold in the Y-axis direction, and the length of the X plate in the Z-axis direction is 99% to 100% of the length of the fixed mold in the Z-axis direction;

[0045] The length of the Y plate in the X-axis direction is 50%~85% of the length of the fixed mold in the X-axis direction, and the length in the Z-axis direction is 99%~100% of the length of the fixed mold in the Z-axis direction;

[0046] The Z 1 Plate and Z 2 The plates are of equal size and are located at the lower ends of the openings on the left and right sides of the fixed mold. 1 Plate and Z 2 The length of the plate in the X-axis direction is 50% to 85% of the length of the fixed mold in the X-axis direction, and the length in the Y-axis direction is 50% to 85% of the length of the fixed mold in the Y-axis direction.

[0047] Four electric screw push rods (X push rod, Y push rod, Z 1 Push rod, Z 2 The push rods are connected to the four push plates and are used to over-compress the compressed object inside the fixed mold and return it to the specified compression position. 1 Pushrod and Z 1 Push plate, Z 2 Pushrod and Z 2 The push plate can be disconnected so that Z 1 Push Plate and Z 2 The push plate is taken out together with the movable mold.

[0048] The electric control system directly controls four electric screw push rods.

[0049] The movable mold is a cube or cuboid with openings on both ends and a hollow interior. The size of the opening on the right end is the same as that of the Z 2 The movable mold is used to transfer the compressed object after being compressed in the fixed mold; the right end opening of the movable mold is connected to the mold surface notch on the negative direction of the Z axis of the fixed mold.

[0050] The lengths of the movable mold in the X-axis direction and the Y-axis direction are 50% to 85% of the lengths of the fixed mold in the X-axis direction and the Y-axis direction, respectively, and the length of the movable mold in the Z-axis direction is 50% to 85% of the length of the fixed mold in the Z-axis direction.

[0051] Because Z 1 Pushrod and Z 1 Push plate, Z 2 Pushrod and Z 2 After the push plate is disconnected, Z 1 Push Plate and Z 2 The push plate may rebound and requires additional rods to fix it. 1 Push Plate and Z 2 Therefore, in addition to containing and transferring the compressed object, the mobile mold also needs 5~20 cm more on the front and back sides (Y axis direction) for installing the plug-in rod to fix the Z 1 Push Plate and Z 2 Push plate.

[0052] After the open-cell foam material is subjected to three-axis compression in the hollow inner space formed by the fixed mold and four push plates, it is pushed into the detachable movable mold. 1 Push Plate and Z 2 The push plate is taken out together.

[0053] After triaxial compression, the moving mold containing the compressed foam is heated and cooled.

[0054] Heating and cooling times increase with the size and thickness of the product.

[0055] After cooling, the material is taken out from the movable mold to obtain the large-size open-cell negative Poisson's ratio foam of the present invention.

[0056] The following examples and comparative examples were all prepared using the above equipment.

[0057] Example 1

[0058] Polyurethane open-cell foam (B30 from Zhongsheng Sponge Products Factory) was cut into cubes of 500 mm × 500 mm × 500 mm, and then placed in the space surrounded by the fixed mold and push plate of the triaxial compression equipment, where the X plate area is 498 mm × 498 mm (the gap between the push plate and the fixed mold is 1 mm on both sides), the Y plate area is 498 mm × 423 mm, and the Z plate area is 498 mm × 423 mm. 1 Plate and Z 2 The area of ​​the plate is 423mm×423mm, and the space enclosed by the fixed mold and the push plate of the three-axis compression equipment is 500mm×500mm×500mm. Start the three-axis compression equipment (such as Figure 1 , Figure 1Schematic diagram of the device), first the X plate of the device compresses downward until the remaining length of the foam in the X-axis direction is 225mm and stops, and its excess compression ratio is 40%, and then the X plate retracts until the remaining length of the foam in the X-axis direction is 425mm and stops, and it retracts to the specified compression ratio, which is 85%;

[0059] Then the Y plate of the equipment compresses forward until the remaining length of the foam in the Y-axis direction is 225 mm and stops, and its excess compression ratio is 40%. Then the Y plate retracts until the remaining length of the foam in the Y-axis direction is 425 mm and stops, and it retracts to the specified compression ratio, which is 85%.

[0060] After Z 1 Plate, Z 2 Plate in Z 1 Push rod, Z 2 Under the control of the push rod, move to the left at the same time to push the foam into the mobile mold. The size of the mobile mold is 425mm (X-axis direction) × 425mm (X-axis direction) × 525mm (Z-axis direction, 425mm+100mm (100 mm indicates the installation of the plug rod to fix the Z 1 Push Plate and Z 2 The moving mold space left by the push plate)), when Z 2 The plate moves to the left and stops at a position 50 mm from the left opening of the moving die, and maintains the position. 1 The plate continues to move to the left until the foam stops at a length of 225 mm in the Z-axis direction, with an excess compression ratio of 40%. 1 The plate is retracted to the remaining 425mm of the foam Z-axis length and stops. It is retracted to the specified compression rate, which is 85%; fix the Z through the convenient jack 1 Plate and Z 2 The distance between the two side holes and the left and right edges of the moving mold are 50mm respectively; then disconnect the Z 1 Plate, Z 2 Plate and Z 1 Push rod, Z 2 Connection of push rod; wait for Z 1 Push rod, Z 2 After the push rod retracts, the moving mold together with the compressed foam and Z 1 Plate, Z 2 The plates were removed together, placed in an oven at 180°C, heated for 6 hours, and then taken out and cooled to room temperature; the foam was removed to obtain a negative Poisson's ratio foam material.

[0061] The negative Poisson's ratio material is tested for Poisson's ratio and density difference. The average tensile initial Poisson's ratio of the negative Poisson's ratio foam material is -0.2. The negative Poisson's ratio foam material is sliced, and the absolute value of the tensile initial Poisson's ratio difference between the skin layer and the core layer is <0.1. The density difference (δ) of the negative Poisson's ratio foam material is ≤20%. Where ρ max and ρ min The local maximum density and local minimum density of the negative Poisson's ratio foam are respectively calculated, ρ ave is the average density of the foam with negative Poisson's ratio.

[0062]

[0063] Figure 4 This is a scanning electron microscope photograph of the polyurethane negative Poisson's ratio foam prepared in Example 1, indicating that the polyurethane negative Poisson's ratio foam has good performance uniformity.

[0064] Example 2

[0065] Polyurethane open-cell foam (B30 from Zhongsheng Sponge Products Factory) was cut into cubes of 1000mm×1500mm×2500mm, and then placed in the space surrounded by the fixed mold and push plate of the triaxial compression equipment, where the X plate area is 2490mm×1490mm (the gap between the push plate and the fixed mold is 5mm on both sides), the Y plate area is 2490mm×840mm, and the Z plate area is 2490mm×840mm. 1 Plate and Z 2 The area of ​​the plates is 840mm×890mm. The space enclosed by the fixed mold and the push plate of the three-axis compression equipment is 1000mm (X-axis direction)×1500mm (Y-axis direction)×2500mm (Z-axis). First, the X-plate of the equipment compresses downward to the remaining 450mm of the foam in the X-axis direction and stops. The excess compression ratio is 40%. Then the X-plate retracts to the remaining 850mm of the foam in the X-axis direction and stops. It retracts to the specified compression ratio, which is 85%.

[0066] Then the Y plate of the equipment compresses forward until the remaining length of the foam in the Y-axis direction is 600mm and stops, and its excess compression ratio is 20%. Then the Y plate retracts until the remaining length of the foam in the Y-axis direction is 900mm and stops, and it retracts to the specified compression ratio, which is 60%;

[0067] After Z 1 Plate, Z 2 Plate in Z 1 Push rod, Z 2 Under the control of the push rod, move to the left at the same time to push the foam into the mobile mold. The size of the mobile mold is 850mm (X-axis direction) × 900mm (X-axis direction) × 1450mm (Z-axis direction, 1250mm+200mm). 2The plate moves to the left and stops at a position 100 mm from the left opening of the moving die, and maintains the position. 1 The plate continues to move to the left until the foam stops at a remaining length of 1000 mm in the Z-axis direction, with an excess compression ratio of 10%. 1 The plate is retracted to the remaining 1250mm of the foam Z-axis length and stops. It is retracted to the specified compression rate, which is 50%; fix the Z through the convenient jack 1 Plate and Z 2 The distance between the two side holes and the left and right edges of the moving mold are 100mm respectively; then disconnect Z 1 Plate, Z 2 Plate and Z 1 Push rod, Z 2 Connection of push rod; wait for Z 1 Push rod, Z 2 After the push rod retracts, the moving mold together with the compressed foam and Z 1 Plate, Z 2 The plates were removed together, placed in an oven at 160°C, heated for 12 hours, and then taken out and cooled to room temperature; the foam was removed to obtain a negative Poisson's ratio foam material.

[0068] The negative Poisson's ratio material is tested for Poisson's ratio, and the average tensile initial Poisson's ratio of the negative Poisson's ratio foam material is -0.3. The negative Poisson's ratio foam material is sliced, and the absolute value of the difference in tensile initial Poisson's ratio between the skin layer and the core layer is ≤0.2. The density difference (δ) of the negative Poisson's ratio foam material is ≤30%.

[0069] Example 3

[0070] Melamine open-cell foam (Puyang Lvyu New Material Technology Co., Ltd., density 10kg / m 3 ) into a cube of 200 mm × 200 mm × 200 mm, and then put it into the mold of the triaxial compression device, and start the triaxial compression device (such as Figure 1 , Figure 1 Schematic diagram of the device), first the X plate of the device compresses downward until the remaining length of the foam in the X-axis direction is 76mm and stops, and its excess compression ratio is 20%, and then the X plate retracts until the remaining length of the foam in the X-axis direction is 116mm and stops, and it retracts to the specified compression ratio, which is 58%;

[0071] Then the Y plate of the device compresses forward until the remaining length of the foam in the Y-axis direction is 76 mm and stops, and its excess compression ratio is 20%. Then the Y plate retracts until the remaining length of the foam in the Y-axis direction is 116 mm and stops, and it retracts to the specified compression ratio, which is 58%.

[0072] After Z 1 Plate, Z 2 Plate in Z1 Push rod, Z 2 Under the control of the push rod, move to the left at the same time to push the foam into the mobile mold. The size of the mobile mold is 116mm (X-axis direction) × 116mm (X-axis direction) × 166mm (Z-axis direction, 116mm+50mm). 2 The plate moves to the left and stops 25mm away from the left opening of the moving die, and maintains the position. 1 The plate continues to move to the left until the foam stops at a length of 76 mm in the Z-axis direction, with an excess compression ratio of 20%. 1 The plate is retracted to the remaining 116mm of the foam Z-axis length and stops. It is retracted to the specified compression rate, which is 58%; fix the Z through the convenient jack 1 Plate and Z 2 The distance between the two side jacks and the left and right edges is 25mm respectively; then disconnect the Z 1 Plate, Z 2 Plate and Z 1 Push rod, Z 2 Connection of push rod; wait for Z 1 Push rod, Z 2 After the push rod retracts, the moving mold together with the compressed foam and Z 1 Plate, Z 2 The plates were removed together, placed in an oven at 220° C., heated for 1 hour, and then taken out and cooled to room temperature; the foam was removed to obtain a melamine negative Poisson's ratio foam material.

[0073] The negative Poisson's ratio material is tested for Poisson's ratio, and the average tensile initial Poisson's ratio of the negative Poisson's ratio foam material is -0.6. The negative Poisson's ratio foam material is sliced, and the absolute value of the difference in tensile initial Poisson's ratio between the skin layer and the core layer is <0.2. The density difference (δ) of the negative Poisson's ratio foam material is ≤20%.

[0074] Example 4

[0075] Polyimide open-cell foam (Puyang Lvyu New Material Technology Co., Ltd., density 30kg / m 3 ) into a cube of 500mm×500mm×500mm, and then put it into the mold of the triaxial compression device, and start the triaxial compression device (such as Figure 1 , Figure 1 Schematic diagram of the device), first the X plate of the device compresses downward until the remaining length of the foam in the X-axis direction is 195mm and stops, and its excess compression ratio is 30%, and then the X plate retracts until the remaining length of the foam in the X-axis direction is 345mm and stops, and it retracts to the specified compression ratio, which is 69%;

[0076] Then the Y plate of the device compresses forward until the remaining length of the foam in the Y-axis direction is 195 mm and stops, and its excess compression ratio is 30%. Then the Y plate retracts until the remaining length of the foam in the Y-axis direction is 345 mm and stops, and it retracts to the specified compression ratio, which is 69%;

[0077] After Z 1 Plate, Z 2 Plate in Z 1 Push rod, Z 2 Under the control of the push rod, move to the left at the same time to push the foam into the mobile mold. The size of the mobile mold is 345mm (X-axis direction) × 345mm (X-axis direction) × 445mm (Z-axis direction, 345mm+100mm). 2 The plate moves to the left and stops at a position 50 mm from the left opening of the moving die, and maintains the position. 1 The plate continues to move to the left until the foam stops at a length of 195 mm in the Z-axis direction, with an excess compression ratio of 30%. 1 The plate is retracted to the remaining 345mm of the foam Z-axis length and stops. It is retracted to the specified compression rate, which is 69%; fix the Z through the convenient jack 1 Plate and Z 2 The distance between the two side sockets and the left and right edges is 50mm respectively; then disconnect the Z 1 Plate, Z 2 Plate and Z 1 Push rod, Z 2 Connection of push rod; wait for Z 1 Push rod, Z 2 After the push rod retracts, the moving mold together with the compressed foam and Z 1 Plate, Z 2 The plates were removed together, placed in an oven at 260° C., heated for 4 hours, and then taken out and cooled to room temperature; the foam was removed to obtain a melamine negative Poisson's ratio foam material.

[0078] The negative Poisson's ratio material is tested for Poisson's ratio, and the average tensile initial Poisson's ratio of the negative Poisson's ratio foam material is -0.4. The negative Poisson's ratio foam material is sliced, and the absolute value of the difference in tensile initial Poisson's ratio between the skin layer and the core layer is <0.15. The density difference (δ) of the negative Poisson's ratio foam material is ≤15%.

[0079] Comparative Example 1

[0080] Polyurethane open-cell foam (B30 from Zhongsheng Sponge Products Factory) was cut into cubes of 500 mm × 500 mm × 500 mm, and then placed in the space surrounded by the fixed mold and push plate of the triaxial compression equipment, where the X plate area is 498 mm × 498 mm (the gap between the push plate and the fixed mold is 1 mm on both sides), the Y plate area is 498 mm × 423 mm, and the Z plate area is 498 mm × 423 mm. 1 Plate and Z 2 The area of ​​the plate is 423mm×423mm, and the space enclosed by the fixed mold and the push plate of the three-axis compression equipment is 500mm×500mm×500mm. Start the three-axis compression equipment (such as Figure 1 , Figure 1 Schematic diagram of the equipment), first the X plate of the equipment compresses downward until the remaining length of the foam in the X-axis direction is 400mm and stops, and its excess compression ratio is 5%, then the X plate retracts until the remaining length of the foam in the X-axis direction is 425mm and stops, and it retracts to the specified compression ratio, which is 85%;

[0081] Then the Y plate of the equipment compresses forward until the remaining length of the foam in the Y-axis direction is 400mm and stops, and its excess compression ratio is 5%. Then the Y plate retracts until the remaining length of the foam in the Y-axis direction is 425mm and stops, and it retracts to the specified compression ratio, which is 85%;

[0082] After that, the Z1 plate and the Z2 plate, under the control of the Z1 push rod and the Z2 push rod, move to the left at the same time to push the foam into the mobile mold. The size of the mobile mold is 425mm (X-axis direction) × 425mm (X-axis direction) × 525mm (Z-axis direction, 425mm+100mm). When the Z2 plate moves to the left and stops at a distance of 50mm from the left end of the mobile mold opening, and maintains the position, the Z1 plate continues to move to the left until the foam stops at a remaining length of 400mm in the Z-axis direction. The excess compression ratio is 5%, and then the Z1 plate returns to the foam Z It stops at the remaining 425mm of the axial length and returns to the specified compression rate, which is 85%; fix the Z1 plate and the Z2 plate through the convenient sockets, and the sockets on both sides are 50mm away from the edge of the movable mold; then disconnect the Z1 plate, the Z2 plate from the Z1 push rod, the Z2 push rod respectively; after the Z1 push rod and the Z2 push rod retract, remove the movable mold together with the compressed foam, the Z1 plate and the Z2 plate, put them in an oven at 180℃, heat them for 6 hours, then take them out and cool them to room temperature; remove the foam to obtain a negative Poisson's ratio foam material.

[0083] The negative Poisson's ratio material is tested for Poisson's ratio and density difference. The average tensile initial Poisson's ratio of the negative Poisson's ratio foam material is -0.15. The negative Poisson's ratio foam material is sliced, and the absolute value of the tensile initial Poisson's ratio difference between the skin layer and the core layer is <0.2. The density difference (δ) of the negative Poisson's ratio foam material is ≤35%.

[0084] Comparative Example 2

[0085] Polyurethane open-cell foam (B30 from Zhongsheng Sponge Products Factory) was cut into cubes of 500 mm × 500 mm × 500 mm, and then placed in the space surrounded by the fixed mold and push plate of the triaxial compression equipment, where the X plate area is 498 mm × 498 mm (the gap between the push plate and the fixed mold is 1 mm on both sides), the Y plate area is 498 mm × 423 mm, and the Z plate area is 498 mm × 423 mm. 1 Plate and Z 2 The area of ​​the plate is 423mm×423mm, and the space enclosed by the fixed mold and the push plate of the three-axis compression equipment is 500mm×500mm×500mm. Start the three-axis compression equipment (such as Figure 1 , Figure 1 Schematic diagram of the device), first the X plate of the device compresses downward until the remaining length of the foam in the X-axis direction is 175mm and stops, and its excess compression ratio is 50%, and then the X plate retracts until the remaining length of the foam in the X-axis direction is 425mm and stops, and it retracts to the specified compression ratio, which is 85%;

[0086] Then the Y plate of the equipment compresses forward until the remaining length of the foam in the Y-axis direction is 175mm and stops, and its excess compression ratio is 50%. Then the Y plate retracts until the remaining length of the foam in the Y-axis direction is 425mm and stops, and it retracts to the specified compression ratio, which is 85%;

[0087] After that, the Z1 plate and the Z2 plate, under the control of the Z1 push rod and the Z2 push rod, move to the left at the same time to push the foam into the mobile mold. The size of the mobile mold is 425mm (X-axis direction) × 425mm (X-axis direction) × 525mm (Z-axis direction, 425mm+100mm). When the Z2 plate moves to the left and stops at a distance of 50mm from the left end of the mobile mold opening, and maintains its position, the Z1 plate continues to move to the left until the foam stops at a remaining length of 175mm in the Z-axis direction. The excess compression ratio is 50%, and then the Z1 plate returns to the foam Z It stops at the remaining 425mm of the axial length and returns to the specified compression rate, which is 85%; fix the Z1 plate and the Z2 plate through the convenient sockets, and the sockets on both sides are 50mm away from the edge of the movable mold; then disconnect the Z1 plate, the Z2 plate from the Z1 push rod, the Z2 push rod respectively; after the Z1 push rod and the Z2 push rod retract, remove the movable mold together with the compressed foam, the Z1 plate and the Z2 plate, put them in an oven at 180℃, heat them for 6 hours, then take them out and cool them to room temperature; remove the foam to obtain a negative Poisson's ratio foam material.

[0088] Due to excessive compression, the foam is compressed too violently, resulting in many damages and cracks inside the foam, making it difficult to obtain a good negative Poisson's ratio foam.

[0089] In summary, the large-size open-cell negative Poisson's ratio foam prepared by the preparation method of the present invention has more uniform performance stability. The preparation method provides a new idea for solving the problem of uneven performance of large-size open-cell negative Poisson's ratio foam products.

[0090] The above embodiments are only used to help understand the method and core idea of ​​the present invention. It should be noted that, for those skilled in the art, several improvements and modifications can be made to the present invention without departing from the principles of the present invention, and these improvements and modifications also fall within the scope of protection of the claims of the present invention.

Claims

1. A method for preparing large-size open-cell negative Poisson's ratio foam, characterized in that: The following steps are involved: The open-cell foam is subjected to triaxial compression, heating, and cooling to obtain a large-size open-cell negative Poisson's ratio foam; The three-axis compression is to perform over-compression and return to the specified compression amount position along the X-axis, Y-axis and Z-axis directions respectively; The excess compression ratio is independently selected from 10% to 40%; The compression ratios at the designated compression positions are independently selected from 50% to 85%.

2. The preparation method according to claim 1, characterized in that: The open-cell foam is selected from polyurethane foam, melamine foam or polyimide foam.

3. The preparation method according to claim 1, characterized in that: The heating temperature is 160 o C ~260 o C; The heating time is 1 to 12 h.

4. The preparation method according to claim 1, characterized in that: The cooling is cooling to 0 o C ~30 o C.

5. The preparation method according to claim 1, characterized in that: The open-cell foam is in a rectangular shape, and the lengths of the three sides are independently selected from 0.2 to 2.5 m.

6. The preparation method according to claim 1, characterized in that: The ratio of the longest side to the shortest side of the open-cell foam is ≤3.

7. A large-size open-cell negative Poisson's ratio foam material, characterized in that: The method is prepared according to any one of claims 1 to 6.

8. The large-size open-cell negative Poisson's ratio foam material according to claim 7, characterized in that: The absolute value of the difference in initial Poisson's ratio between the skin layer and the core layer of the large-size open-cell negative Poisson's ratio foam material during stretching is ≤0.

2.

9. The large-size open-cell negative Poisson's ratio foam material according to claim 7 or 8, characterized in that: The density difference of the large-size open-cell negative Poisson's ratio foam material is ≤30%.

10. The large-size open-cell negative Poisson's ratio foam material according to claim 9, characterized in that: The three-side dimensions of the large-size open-cell negative Poisson's ratio foam material are independently selected from 0.1 to 2.125 m.