Inner liner rubber for all-steel radial tire of heavy truck

By using low-cost raw materials and optimized proportions in the airtight layer glue formula of all-steel radial tires of heavy-duty trucks, the problem of high manufacturing costs is solved, and the effect of reducing production costs and improving flexural performance is achieved.

CN118909321APending Publication Date: 2024-11-08刘琦
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411068545.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The manufacturing cost of all-steel radial tires of heavy-duty trucks is generally high, which has brought economic pressure to tire manufacturers.

Method used

By using a small amount of low-cost raw materials such as butyl recycled glue, light calcium carbonate, air blocker, and high-active zinc oxide in the formulation design of airtight layer glue, and optimizing the glue system, filling and reinforcing system, softening and plasticizing The component ratio of the system is to eliminate the high-cost vulcanizing agent DTDM, and a semi-effective vulcanizing system with a main accelerator NS and a small amount of auxiliary accelerator DM to reduce production costs.

Benefits of technology

While ensuring that the air-tight layer glue is not reduced, the production cost of air-tight layer glue for heavy-duty trucks is reduced, the flexural performance is improved, and the production cost of mixing glue per kilogram is saved is 0.45 yuan per kilogram of mixed glue. A production of 1 million tires can save 1.8 million yuan.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The raw rubber system, the filling and reinforcing system, the softening and plasticizing system and the vulcanization system of the airtight layer rubber formula of the all-steel radial tire of the heavy truck are subjected to optimization adjustment and experimental verification, the production cost of the finally optimized experimental formula is reduced, and part of physical and mechanical properties of the rubber compound are improved. The method lays a foundation for cost reduction and benefit increase of tire manufacturing enterprises.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention patent relates to the manufacturing field of heavy-duty truck all-steel radial tires, and relates to an airtight layer rubber for heavy-duty truck all-steel radial tires with good performance and low cost. Background Art

[0002] At present, the manufacturing cost of heavy-duty truck all-steel radial tires is generally high, and the high manufacturing cost has brought great economic pressure to tire manufacturers. In order to alleviate the economic pressure of tire manufacturers, the present invention reduces the production cost of the airtight layer rubber of heavy-duty truck all-steel radial tires to achieve the purpose of reducing costs for tire manufacturers.

[0003] According to the design characteristics of the heavy-duty truck all-steel radial tire itself, the production cost of the air-inner layer rubber formula is first considered when designing the formula of the air-inner layer rubber. By replacing a small amount of low-cost raw materials and rationally matching the added components of different raw materials, the production cost of the designed formula is reduced while ensuring that the air retention performance of the air-inner layer rubber formula is not reduced. The low-cost air-inner layer rubber of the heavy-duty truck all-steel radial tire is beneficial to tire manufacturing companies in reducing costs and increasing efficiency. Summary of the invention

[0004] The patent of the present invention uses low-priced raw materials such as butyl recycled rubber, light calcium carbonate, air retarder, and highly active zinc oxide through a small amount of substitution method to reduce the unit kilogram cost of the airtight layer rubber formula of the heavy-duty truck all-steel radial tire; by optimizing the component ratio of different raw materials in the raw rubber system, the filling and reinforcement system, the softening and plasticizing system, and the vulcanization system, it ensures that the physical and mechanical properties of the airtight layer rubber of the heavy-duty truck all-steel radial tire are not reduced, and at the same time, the reasonable raw material component ratio also improves the flexural performance of the airtight layer rubber of the heavy-duty truck all-steel radial tire.

[0005] By optimizing the component ratio of each system in the airtight layer rubber formula and comparing and verifying the physical and mechanical properties of the mixed rubbers of different systems, the airtight layer rubber formula with good performance and low cost is selected. The preferred formula uses natural rubber and brominated butyl rubber, while increasing the amount of butyl reclaimed rubber, eliminating the use of high-cost vulcanizing agent DTDM, and adopting a semi-effective vulcanization system with a main accelerator NS and a small amount of auxiliary accelerator DM.

[0006] The specific implementation scheme, experimental process and test results of the patent of this invention are as follows: 1 Experiment 1.1 Main Raw Materials

[0007] Natural rubber: brand TSR9710, Xishuangbanna Sinochem Rubber Co., Ltd.; Bromobutyl rubber: brand 2302, Zhejiang Xinhui New Materials Co., Ltd.; Modified chlorosulfonated polyethylene: brand MCSM, Taizhou Huangyan Donghai Chemical Co., Ltd.; Butyl reclaimed rubber: Hebei Quzhou Junteng Rubber New Material Technology Co., Ltd.; Carbon black: brand N660, Yunnan Yunwei Feihu Chemical Co., Ltd.; Aromatic oil: Sichuan Chengdu Dasen Petrochemical Co., Ltd.; Highly active zinc oxide: Sichuan Dongfang Tiantai Alloy Co., Ltd.; Stearic acid: brand 800, Dongguan Yihai Oil Chemical Industry Co., Ltd.; Tert-octyl phenolic tackifying resin: brand SL1801, Huaqi (China) Chemical Co., Ltd.; Homogenizer: brand SL-400, Huaqi (China) Chemical Co., Ltd.; Sulfur powder: Sichuan Chenhui Chemical Co., Ltd.; Accelerator: brand DM, Shandong Shangshun Chemical Co., Ltd.; Accelerator: brand NS, Shandong Yanggu Huatai Co., Ltd.; Vulcanizing agent: brand DTDM, Anhui Puyang Weilin Chemical Co., Ltd. 1.2 Test formula

[0008] Through multiple rounds of comparative tests, the optimized formulas of airtight layers 1# to 7# shown in Table 1 were obtained, 8# is the reference formula, and small and large formula experimental tests were carried out on the following formulas to determine the final optimized formula.

[0009] 1.3 Main equipment and instruments

[0010] Kobe Steel, Ltd., Japan: BB-2 type internal mixer, BB430 type internal mixer; Qingdao Xianrui Electromechanical Co., Ltd.: XK-160 type open mixer, XLB-800 type flat vulcanizer; Yiyang Rubber Machinery Co., Ltd.: GN255 type internal mixer, XK-660 type open mixer; Alpha Corporation, USA: Mooney viscometer MV2000, rotorless vulcanometer MD2000; Instron Corporation, USA: 3365 type electronic tensile testing machine; Jinan Languang Electromechanical Technology Co., Ltd.: VAC-V2 differential pressure gas permeability instrument; High Speed ​​Rail (Taiwan) Testing Instrument Co., Ltd.: vulcanized rubber flexural test machine. 1.4 Sample preparation

[0011] Small compounding experiment: BB-2 type internal mixer and XK-160 type open mixer were used to mix and prepare the sample. First, mix in the internal mixer, and add the following materials: raw rubber / drug (speed 70r·min -1 , pressing 40 seconds) → carbon black / aromatic oil (speed 60r·min -1, press the roller for 60 seconds) → lift the roller and hold for 10 seconds → press the roller for 300 seconds or remove the glue at 130℃, use the open mill to pass the thin film 5 times, and leave it for 2 hours. Add the sulfur-promoting system on the open mill (roller temperature 60±5℃), and after the drug is completely absorbed, make 8 triangle packs to make the film, and leave it for 8 hours. The sample is vulcanized on the XLB-800 flat vulcanizer (vulcanization conditions: 151℃*40min).

[0012] Large-scale compounding experiment: BB430 and GN255 internal mixers were used to prepare samples by mixing in sections. Plasticized rubber (raw rubber plasticizing), masterbatch chemicals, aromatic oil and 3 / 4 carbon black were added to the BB430 internal mixer for mixing (rotor speed: 50rpm, upper top bolt pressure: 18Mpa, mixing time: 170s) to prepare a first-stage masterbatch, which was left for 2 hours. The first-stage masterbatch and 1 / 4 carbon black were added to the BB430 internal mixer for mixing (rotor speed: 40rpm, upper top bolt pressure: 18Mpa, mixing time: 130s) to prepare a second-stage masterbatch, which was left for 2 hours. The second-stage masterbatch and the sulfur-promoting system were added to the GN255 internal mixer for mixing (rotor speed: 30rpm, upper top bolt pressure: 13Mpa, mixing time: 135s) to prepare the final rubber, which was left for 8 hours. The samples were cut for vulcanization, and the vulcanization conditions were the same as above. 1.5 Performance Testing

[0013] All properties of rubber are tested in accordance with the relevant national or enterprise standards. 2 Results and discussion 2.1 Small coordination experiment results

[0014] The relevant performance tests of the mixed rubber and the vulcanized rubber are shown in Table 1 and Table 2.

[0015]

[0016] Table 1 shows that there is no significant difference in Mooney viscosity between the experimental formula and the reference formula; the scorch time of the experimental formula 1 t 5 The longest scorch time of 5# test formula and 8# reference formula t 5 Close to; 8# reference formula maximum torque MH maximum, positive vulcanization time t 90 The longest, the maximum torque MH of the 4# test formula and the positive vulcanization time of the 5# test formula t 90 Second; the sulfur conversion time of 5# test formula Rev3 Closer to reference formula 8#.

[0017]

[0018] Table 2 shows that the tensile strength, elongation at break, tear strength and flexure times of the 5# experimental formula are significantly better than those of the other experimental formulas and the 8# reference formula; the aging coefficient of the 8# reference formula is the largest, followed by the 5# experimental formula; there is no significant difference in other physical and mechanical properties between the experimental formula and the reference formula.

[0019] Through the results of small-scale experiments, the 5# test formula was selected as the best airtight layer formula. In order to further improve the physical and mechanical properties of the 5# test formula, the formula was optimized and adjusted to determine the 6#~7# test formulas. Large-scale experiments were conducted to verify the 6#~7# test formulas and the 8# reference formula. 2.2 Results of large-scale matching experiments

[0020] The relevant performance tests of the mixed rubber and vulcanized rubber are shown in Table 3 and Table 4.

[0021]

[0022] Table 3 shows that there is no significant difference in Mooney viscosity between the test formula and the reference formula; the scorch time of the 7# test formula t 5 The longest; the positive curing time of 7# test formula and 8# reference formula t 90 Close to; 7# test formula sulfur conversion return time Rev3 longest.

[0023]

[0024] Table 4 shows that: the hardness of the 8# reference formula is the largest, and the hardness of the 6# and 7# test formulas is close; the 100% and 300% elongation strength of the 8# reference formula is the largest, and the 100% and 300% elongation strength of the 6# and 7# test formulas are close; the tensile strength, tear strength, flexure times, carbon black dispersion and aging coefficient of the 7# test formula are significantly better than those of the 6# test formula and the 8# reference formula, and there is no obvious difference in gas permeability and air permeability coefficient between the test formula and the reference formula.

[0025] Through multiple rounds of small- and large-combination test results verification, the 7# test formula was finally selected as the best airtight layer rubber formula for heavy-duty truck all-steel radial tires. 2.3 Rubber compounding cost calculation

[0026] According to the latest raw material prices, the 7# test formula saves 0.45 yuan per kilogram of mixed rubber compared to the 8# reference formula. The use of the 7# test formula in the airtight layer rubber of heavy truck all-steel radial tires can save 1.8 million yuan in production costs for tire manufacturers every year, based on an annual production of 1 million 12.00R20 tires. 3 Conclusion

[0027] By continuously optimizing and adjusting the test formula and verifying the physical properties, we finally selected the airtight layer rubber formula of heavy-duty truck all-steel radial tires with relatively excellent performance. The production cost of the new formula is 0.45 yuan / kg lower than that of the reference formula. This patent has laid a foundation for tire manufacturers to reduce costs and increase efficiency.

Claims

1. Claim 1: An airtight layer adhesive for a heavy truck all-steel radial tire, comprising low-cost raw materials of butyl reclaimed rubber, light calcium carbonate, air retarder, and highly active zinc oxide, and ensuring stable performance of the airtight layer adhesive by optimizing the component ratio of different types of raw materials.

2. The airtight layer adhesive for heavy truck all-steel radial tire according to claim 1, characterized in that: 35 parts of butyl reclaimed rubber were used to replace 10 parts of bromobutyl rubber.

3. The airtight layer rubber for heavy truck all-steel radial tire according to claim 1, characterized in that: Use 20 parts of light calcium carbonate.

4. The airtight layer rubber for heavy truck all-steel radial tire according to claim 1, characterized in that: Use 10 parts air blocker.

5. The airtight layer rubber for heavy truck all-steel radial tire according to claim 1, characterized in that: Use 7 parts of aromatic oil.

6. The airtight layer rubber for heavy truck all-steel radial tire according to claim 1, characterized in that: Use 3 parts of highly active zinc oxide instead of 3.8 parts of zinc oxide-80.

7. The airtight layer rubber for heavy truck all-steel radial tire according to claim 1, characterized in that: 0.9 parts of sulfur powder, 0.7 parts of accelerator NS, and 0.2 parts of accelerator DM are used instead of 0.8 parts of sulfur powder, 0.4 parts of vulcanizing agent DTDM, and 0.8 parts of accelerator DM.