Rubber sole and preparation method thereof

By using sheet-like inorganic filler and island-like carbon-encapsulated layer in rubber soles, combined with the three-dimensional filling structure of carbonized bagasse fibers, the problem of inorganic filler migration is solved, and the mechanical properties and service life of rubber soles are improved.

CN118909323AInactive Publication Date: 2024-11-08WENZHOU QIJIA SHOES CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411331931.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-24
Publication Date
2024-11-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

During the processing process, the filler migration is caused by the interface incompatibility between the inorganic filler and the organic rubber matrix, which affects the product performance and service life.

Method used

A sheet-like inorganic filler is used and an island-like carbon-encapsulated layer is formed on its surface, and a carbide bagasse fiber is combined to form a three-dimensional fill structure, which enhances the interaction force of the rubber material and limits the migration of the filler.

Benefits of technology

It improves the interaction force between filler and rubber, reduces filler migration, extends the service life of the product, and maintains good mechanical properties under aging conditions.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention belongs to the technical field of high polymer materials. The invention relates to a sole, in particular to a rubber sole and a preparation method thereof. The product provided by the invention comprises natural rubber and a flaky inorganic filler dispersed in the natural rubber, wherein the use amount of the flaky inorganic filler is 6.5-8.5% of the mass of the natural rubber; a carbon-coated layer is arranged on the surface of the sheet-shaped inorganic filler, and the carbon-coated layer coats the surface of the inorganic filler in an island shape. Wherein the carbon coating of the sheet-shaped inorganic filler comprises the following steps: mixing the sheet-shaped inorganic filler and a starch solution, adding an emulsifier, uniformly stirring and mixing, carrying out suction filtration, drying, dispersing, transferring to an inert gas protection state, and heating for carbonization, so as to form an island-shaped carbon coating layer on the surface of the sheet-shaped inorganic filler. The obtained product can effectively inhibit migration of the filler, and the service life of the rubber sole is prolonged.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of polymer materials and more specifically relates to a rubber sole and a preparation method thereof. Background Art

[0002] Rubber material is a common material in the sole manufacturing process. It has good elasticity and wear resistance. Although it is a relatively mature application, there are still some bottleneck problems.

[0003] For example, some problems in the rubber vulcanization process. Vulcanization is an important part of the rubber processing process. The length of the vulcanization time, the temperature and the amount of vulcanizer used will affect the quality and performance of the rubber sole. For example, too long a vulcanization time may increase the fluidity of the rubber in the mold, while insufficient vulcanization time may cause insufficient sulfur spraying.

[0004] In addition, due to the influence of moisture, warm air or ozone, rubber soles will age, causing the color of the sole surface to change, affecting the appearance of the sole. Summary of the invention

[0005] The technical problem to be solved by the present invention is: for rubber soles, inorganic fillers are added for reinforcement, but due to the general interface compatibility between the inorganic fillers and the organic rubber matrix, the fillers migrate during processing or use, resulting in a gradual decline in product performance, which ultimately affects the service life of the product. The present invention provides a rubber sole and a preparation method thereof.

[0006] The purpose of the present invention is to provide a rubber sole.

[0007] Another object of the present invention is to provide a method for preparing a rubber sole.

[0008] The above-mentioned purpose of the present invention is achieved through the following technical solutions:

[0009] A rubber sole comprising natural rubber and a flake inorganic filler dispersed in the natural rubber;

[0010] Wherein, the amount of the flaky inorganic filler is 6.5-8.5% of the mass of the natural rubber;

[0011] The surface of the flaky inorganic filler is provided with a carbon coating layer, and the carbon coating layer covers the surface of the inorganic filler in an island shape.

[0012] Preferably, the flaky inorganic filler is selected from any one of flaky aluminum oxide, flaky magnesium oxide and flaky zinc oxide.

[0013] Preferably, the coating amount of the carbon coating layer is 6-8% of the mass of the flaky inorganic filler.

[0014] Preferably, the D50 of the flaky inorganic filler is 65-85 μm; and the particle size distribution range of the flaky inorganic filler is 20-150 μm.

[0015] Preferably, the rubber sole further comprises carbonized bagasse fiber;

[0016] The amount of the carbonized bagasse fiber is 2.2-2.5% of the mass of the natural rubber;

[0017] Furthermore, silicon dioxide is continuously deposited in at least a portion of the internal pores and the surface of the carbonized bagasse fiber;

[0018] The deposited amount of silicon dioxide accounts for 25-30% of the total mass of the carbonized bagasse fiber.

[0019] The above technical solution further introduces carbonized bagasse fibers, and silicon dioxide is continuously deposited in the internal pores and surface of the carbonized bagasse fibers. In this way, the carbonized bagasse fibers have a certain rigidity, so that they cooperate with the aforementioned flaky inorganic fillers to form a three-dimensional filling of the rubber material. In particular, the fibers can form an interlocking network with the three-dimensional network structure formed after the rubber is vulcanized, thereby effectively confining the flaky inorganic fillers therein. The introduction of carbonized bagasse fibers with a certain rigidity avoids the movement of the molecular chains of the rubber after it softens during the temperature rise process, which causes the interlocking network structure to be too easy to deform and causes the migration of the flaky inorganic fillers.

[0020] A method for preparing a rubber sole, the specific preparation steps comprising:

[0021] Carbon coating of flaky inorganic fillers:

[0022] The flaky inorganic filler and the starch solution are mixed, and an emulsifier is added, and after being stirred and mixed evenly, the mixture is filtered, dried, and after being dispersed, transferred to an inert gas protection state, and heated to carbonize to form an island-shaped carbon coating layer on the surface of the flaky inorganic filler;

[0023] Preparation of rubber soles:

[0024] The natural rubber, the flaky inorganic filler with the island-shaped carbon coating layer on the surface, and other additives are mixed and poured into a rubber mixer and mixed evenly to obtain a mixed material;

[0025] The mixed material is then plasticized in a rubber mixer and extruded into rubber strips;

[0026] The rubber strip is then transferred into a mold, hot-pressed, vulcanized, and trimmed to obtain a rubber sole.

[0027] Preferably, the other additives include: sulfur, vulcanization accelerator and antioxidant;

[0028] The vulcanization accelerator is selected from any one of accelerator M, accelerator DM, accelerator MZ, accelerator MTT and accelerator BT;

[0029] The antioxidant is selected from any one of antioxidant 4010, antioxidant RD, antioxidant MB, antioxidant D, antioxidant AW and antioxidant BLE.

[0030] Preferably, the other auxiliary agents also include: carbonized bagasse fiber;

[0031] The preparation steps of the carbonized bagasse fiber include:

[0032] The sugarcane bagasse is steam exploded, washed, dried, and then heat treated at a temperature of 270-280° C. to obtain heat-treated bagasse;

[0033] The heat-treated bagasse, ethyl orthosilicate, anhydrous ethanol and oxalic acid are mixed, heated to reflux reaction, and then filtered, washed and dried to obtain a coating precursor;

[0034] The obtained coated precursor is heated to 780-800° C. under the protection of inert gas and carbonized at high temperature to obtain carbonized bagasse fiber.

[0035] Beneficial effects:

[0036] (1) The technical solution of the present invention adopts a flaky inorganic filler as the main filler. Due to its shape characteristics, it can form a strong interaction with the polymer network structure of natural rubber, especially the network structure after vulcanization. Specifically, compared with conventional spherical or quasi-spherical granular fillers, the irregular edges of the flaky filler can easily make the polymer network structure form a physical interlocking with it, thereby improving the interaction between the filler and the rubber and reducing the migration of the filler;

[0037] (2) In addition, the inventors have found that the use of flaky inorganic fillers, since they are inorganic materials, is easy to agglomerate in the rubber system, and in order to break up the agglomeration, it often takes a longer processing time. By forming a carbon coating layer on the surface of the inorganic filler, not only the direct interface compatibility between the inorganic filler and the organic natural rubber is improved, but also the filler surface can be made more lubricated, which is conducive to the slippage of the flaky structure during the system processing and the mixing of the components. In this way, the processing time can be compressed; and the presence of the carbon coating layer can provide additional thermal stability and reduce the migration of fillers caused by high temperature during the use or storage of the product.

[0038] (3) However, if the carbon coating forms a continuous coating on the surface of the flaky inorganic filler, the density of the flaky filler will be too low. During the processing, it is easy to float on the surface of the system and it is difficult to disperse evenly inside the system. This problem can be effectively solved by island coating. After the island coating, the filler can also obtain a larger specific surface area. In addition, the existence of the island carbon layer can serve as a bonding connection point between the inorganic filler and the organic rubber. DETAILED DESCRIPTION

[0039] The present invention is further described below with reference to specific examples, but the examples do not limit the present invention in any form. Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art.

[0040] Unless otherwise specified, the reagents and materials used in the following examples are commercially available.

[0041] Example 1

[0042] Carbon coating of flaky inorganic fillers:

[0043] The flaky inorganic filler and the starch solution with a mass fraction of 8% are mixed in a mass ratio of 1:8 and poured into a mixer, and an emulsifier OP-10 with a mass fraction of 1% of the flaky inorganic filler is added, and the mixture is stirred and mixed with a stirrer at a speed of 300 r / min for 45 minutes, and then filtered to collect the filter cake, and the obtained filter cake is transferred to an oven, and dried to a constant weight at a temperature of 100° C. to obtain a dry filter cake, and then the obtained dry filter cake is broken up and transferred to a carbonization furnace, and heated to 750° C. in an argon atmosphere, and carbonized for 2 hours, and then cooled and discharged to form an island-shaped carbon coating layer on the surface of the flaky inorganic filler;

[0044] The D50 of the flaky inorganic filler is 65 μm; and the particle size distribution range of the flaky inorganic filler is 20-150 μm;

[0045] The flaky inorganic filler is selected from flaky aluminum oxide;

[0046] By adjusting the mass ratio and concentration of the aforementioned materials and the processing parameters, the coating amount of the carbon coating layer is adjusted to be 6% of the mass of the flaky inorganic filler; wherein the mass of the flaky inorganic filler refers to the mass of the filler before the carbon coating treatment;

[0047] Preparation of Carbonized Bagasse Fiber:

[0048] After mixing bagasse and water in a mass ratio of 1:1, the mixture is transferred into an autoclave, maintained at a temperature of 180°C and a pressure of 2.5 MPa for 5 minutes, and then the pressure relief valve is opened to release the pressure instantly to perform steam explosion. After steam explosion, the mixture is washed with water for 3 times, dried, and then heat-treated in a nitrogen atmosphere at a temperature of 270°C to obtain heat-treated bagasse.

[0049] 90 parts of heat-treated bagasse, 8 parts of ethyl orthosilicate, 200 parts of anhydrous ethanol and 30 parts of oxalic acid were mixed by weight, heated under reflux at 85°C for 1 hour, filtered, and the filter cake was collected, and washed with deionized water for 3 times, and then dried to obtain a coated precursor;

[0050] The obtained coated precursor was heated to 780°C under argon gas protection and carbonized for 3 hours to obtain carbonized bagasse fiber;

[0051] The deposited amount of silicon dioxide accounts for 25% of the total mass of the carbonized bagasse fiber;

[0052] Preparation of rubber soles:

[0053] The natural rubber, the flaky inorganic filler with the island-shaped carbon coating layer on the surface, the carbonized bagasse fiber, the sulfur, the vulcanization accelerator and the antioxidant are mixed and poured into a rubber mixing machine and mixed evenly to obtain a mixed material;

[0054] Wherein, the amount of the flaky inorganic filler having an island-shaped carbon coating layer on the surface is 6.5% of the mass of the natural rubber;

[0055] The amount of the carbonized bagasse fiber is 2.2% of the mass of the natural rubber;

[0056] The amount of sulfur used is 0.3 times the mass of the natural rubber;

[0057] The amount of the vulcanization accelerator is 0.5% of the mass of the natural rubber;

[0058] The dosage of the antioxidant is 0.8% of the mass of the natural rubber;

[0059] The mixed material is then plasticized in a rubber mixer and extruded into rubber strips;

[0060] The rubber strip is then transferred into a mold, hot-pressed, vulcanized for 5 minutes at a temperature of 145°C and a pressure of 0.4 MPa, and trimmed to obtain a rubber sole.

[0061] The vulcanization accelerator is selected from: accelerator M;

[0062] The antioxidant is selected from: antioxidant 4010.

[0063] Example 2

[0064] Carbon coating of flaky inorganic fillers:

[0065] The flaky inorganic filler and the starch solution with a mass fraction of 10% are mixed in a mass ratio of 1:9 and poured into a mixer, and an emulsifier OP-10 with a mass fraction of 1% of the flaky inorganic filler is added, and the mixture is stirred and mixed with a stirrer at a speed of 300 r / min for 45 minutes, and then the mixture is filtered and the filter cake is collected, and the obtained filter cake is transferred to an oven and dried to a constant weight at a temperature of 100° C. to obtain a dry filter cake, and then the obtained dry filter cake is broken up and transferred to a carbonization furnace, and heated to 780° C. in an argon atmosphere, and carbonized for 2 hours, and then cooled and discharged to form an island-shaped carbon coating layer on the surface of the flaky inorganic filler;

[0066] The D50 of the flaky inorganic filler is 75 μm; and the particle size distribution range of the flaky inorganic filler is 20-150 μm;

[0067] The flaky inorganic filler is selected from flaky magnesium oxide;

[0068] By adjusting the mass ratio and concentration of the aforementioned materials and the processing parameters, the coating amount of the carbon coating layer is adjusted to be 7.2% of the mass of the flaky inorganic filler; wherein the mass of the flaky inorganic filler refers to the mass of the filler before the carbon coating treatment;

[0069] Preparation of Carbonized Bagasse Fiber:

[0070] After mixing bagasse and water in a mass ratio of 1:1, the mixture is transferred into an autoclave, maintained at a temperature of 180°C and a pressure of 2.5 MPa for 5 minutes, and then the pressure relief valve is opened to release the pressure instantly to perform steam explosion. After steam explosion, the mixture is washed with water for 4 times, dried, and then heat-treated in a nitrogen atmosphere at a temperature of 275°C to obtain heat-treated bagasse.

[0071] 95 parts of heat-treated bagasse, 10 parts of ethyl orthosilicate, 210 parts of anhydrous ethanol and 32 parts of oxalic acid were mixed by weight, heated under reflux at 85°C for 1.5 hours, filtered, and the filter cake was collected. The filter cake was washed with deionized water for 3 times, and then dried to obtain a coated precursor;

[0072] The obtained coated precursor was heated to 790°C under argon gas protection and carbonized for 3 hours to obtain carbonized bagasse fiber;

[0073] The deposited amount of silicon dioxide accounts for 27% of the total mass of the carbonized bagasse fiber;

[0074] Preparation of rubber soles:

[0075] The natural rubber, the flaky inorganic filler with the island-shaped carbon coating layer on the surface, the carbonized bagasse fiber, the sulfur, the vulcanization accelerator and the antioxidant are mixed and poured into a rubber mixing machine and mixed evenly to obtain a mixed material;

[0076] The amount of the flaky inorganic filler having an island-shaped carbon coating on the surface is 7.2% of the mass of the natural rubber;

[0077] The amount of the carbonized bagasse fiber is 2.4% of the mass of the natural rubber;

[0078] The amount of sulfur used is 0.3 times the mass of the natural rubber;

[0079] The amount of the vulcanization accelerator is 0.5% of the mass of the natural rubber;

[0080] The dosage of the antioxidant is 0.8% of the mass of the natural rubber;

[0081] The mixed material is then plasticized in a rubber mixer and extruded into rubber strips;

[0082] The rubber strip is then transferred into a mold, hot-pressed, vulcanized for 5 minutes at a temperature of 145°C and a pressure of 0.4 MPa, and trimmed to obtain a rubber sole.

[0083] The vulcanization accelerator is selected from: accelerator DM;

[0084] The antioxidant is selected from: antioxidant RD.

[0085] Example 3

[0086] Carbon coating of flaky inorganic fillers:

[0087] The flaky inorganic filler and the starch solution with a mass fraction of 12% are mixed in a mass ratio of 1:10 and poured into a mixer, and an emulsifier OP-10 with a mass fraction of 1% of the flaky inorganic filler is added, and the mixture is stirred and mixed with a stirrer at a speed of 300 r / min for 45 minutes, and then the mixture is filtered and the filter cake is collected, and the obtained filter cake is transferred to an oven and dried to a constant weight at a temperature of 100° C. to obtain a dry filter cake, and then the obtained dry filter cake is broken up and transferred to a carbonization furnace, and heated to 800° C. in an argon atmosphere, and carbonized for 2 hours, and then cooled and discharged to form an island-shaped carbon coating layer on the surface of the flaky inorganic filler;

[0088] The D50 of the flaky inorganic filler is 85 μm; and the particle size distribution range of the flaky inorganic filler is 20-150 μm;

[0089] The flaky inorganic filler is selected from flaky zinc oxide;

[0090] By adjusting the mass ratio and concentration of the aforementioned materials and the processing parameters, the coating amount of the carbon coating layer is adjusted to be 8% of the mass of the flaky inorganic filler; wherein the mass of the flaky inorganic filler refers to the mass of the filler before the carbon coating treatment;

[0091] Preparation of Carbonized Bagasse Fiber:

[0092] After mixing bagasse and water in a mass ratio of 1:1, the mixture is transferred into an autoclave, maintained at a temperature of 180°C and a pressure of 2.5 MPa for 5 minutes, and then the pressure relief valve is opened to release the pressure instantly to perform steam explosion. After steam explosion, the mixture is washed with water for 5 times, dried, and then heat-treated in a nitrogen atmosphere at a temperature of 280°C to obtain heat-treated bagasse.

[0093] 100 parts of heat-treated bagasse, 12 parts of ethyl orthosilicate, 220 parts of anhydrous ethanol and 35 parts of oxalic acid were mixed by weight, heated under reflux at 85°C for 2 hours, filtered, and the filter cake was collected, and washed with deionized water for 3 times, and then dried to obtain a coated precursor;

[0094] The obtained coated precursor was heated to 800°C under argon gas protection and carbonized for 3 hours to obtain carbonized bagasse fiber;

[0095] The deposited amount of silicon dioxide accounts for 30% of the total mass of the carbonized bagasse fiber;

[0096] Preparation of rubber soles:

[0097] The natural rubber, the flaky inorganic filler with the island-shaped carbon coating layer on the surface, the carbonized bagasse fiber, the sulfur, the vulcanization accelerator and the antioxidant are mixed and poured into a rubber mixing machine and mixed evenly to obtain a mixed material;

[0098] Wherein, the amount of the flaky inorganic filler having an island-shaped carbon coating layer on the surface is 8.5% of the mass of the natural rubber;

[0099] The amount of the carbonized bagasse fiber is 2.5% of the mass of the natural rubber;

[0100] The amount of sulfur used is 0.3 times the mass of the natural rubber;

[0101] The amount of the vulcanization accelerator is 0.5% of the mass of the natural rubber;

[0102] The dosage of the antioxidant is 0.8% of the mass of the natural rubber;

[0103] The mixed material is then plasticized in a rubber mixer and extruded into rubber strips;

[0104] The rubber strip is then transferred into a mold, hot-pressed, vulcanized for 5 minutes at a temperature of 145°C and a pressure of 0.4 MPa, and trimmed to obtain a rubber sole.

[0105] The vulcanization accelerator is selected from: accelerator MZ;

[0106] The antioxidant is selected from: antioxidant MB.

[0107] Example 4

[0108] The present embodiment differs from the embodiment 1 in that no ethyl orthosilicate is added, and the other conditions remain unchanged.

[0109] Example 5

[0110] The present embodiment differs from the embodiment 1 in that no carbonized bagasse fiber is added, and the other conditions remain unchanged.

[0111] Comparative Example 1

[0112] The difference between this comparative example and Example 1 is that spherical alumina with a sphericity of 8.0 of the same mass is used to replace the flake alumina for carbon coating, and the other conditions remain unchanged.

[0113] Comparative Example 2

[0114] The difference between this comparative example and Example 1 is that the mass fraction of the starch solution is 20%, the coating amount of the carbon coating layer is 13% of the mass of the flaky inorganic filler, and the other conditions remain unchanged.

[0115] Comparative Example 3

[0116] The difference between this comparative example and Example 1 is that the flaky inorganic filler is not subjected to carbon coating treatment, and the other conditions remain unchanged.

[0117] The performance tests were performed on the products obtained in the examples and comparative examples. The specific test methods and test results are as follows:

[0118] According to GB / T 528-2009 standard, the tensile strength 1 and tear strength 1 of the product were tested; the detailed test results are shown in Table 1;

[0119] Table 1: Product performance test results before aging

[0120] Tensile strength 1 / MPa Tear strength 1 / (KN / m) Example 1 12.2 10.6 Example 2 12.3 10.8 Example 3 12.5 10.9 Example 4 11.8 10.3 Example 5 10.2 9.4 Comparative Example 1 11.6 10.2 Comparative Example 2 11.5 10.0 Comparative Example 3 11.3 9.9

[0121] The products of the above-mentioned embodiments and comparative examples were then placed in an aging box, and aged for 45 days at an ozone concentration of 3%, a temperature of 40°C, and a relative humidity of 75%. After that, the products were taken out and dried, and the tensile strength 2 and tear strength 2 of the products were tested respectively according to the standard GB / T 528-2009. The detailed test results are shown in Table 2.

[0122] Table 2: Product performance test results after aging

[0123] Tensile strength 1 / MPa Tear strength 1 / (KN / m) Example 1 12.0 10.4 Example 2 12.1 10.5 Example 3 12.2 10.6 Example 4 11.4 9.8 Example 5 9.5 8.8 Comparative Example 1 10.7 9.3 Comparative Example 2 10.5 9.1 Comparative Example 3 10.4 8.9

[0124] It can be seen from the test results in Table 1 and Table 2 that the product obtained by the present invention has excellent mechanical properties, and after the simulated aging experiment, it can still maintain good mechanical properties, effectively extending the service life of the product.

[0125] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.

Claims

1. A rubber sole, characterized in that: Comprising natural rubber, and flake inorganic filler dispersed in the natural rubber; Wherein, the amount of the flaky inorganic filler is 6.5-8.5% of the mass of the natural rubber; The surface of the flaky inorganic filler is provided with a carbon coating layer, and the carbon coating layer covers the surface of the inorganic filler in an island shape.

2. A rubber sole according to claim 1, characterized in that: The flaky inorganic filler is selected from any one of flaky aluminum oxide, flaky magnesium oxide and flaky zinc oxide.

3. A rubber sole according to claim 1, characterized in that: The coating amount of the carbon coating layer is 6-8% of the mass of the flaky inorganic filler.

4. A rubber sole according to claim 1, characterized in that: The D50 of the flaky inorganic filler is 65-85 μm; and the particle size distribution range of the flaky inorganic filler is 20-150 μm.

5. The rubber sole according to claim 1, characterized in that: The rubber sole also includes carbonized bagasse fiber; The amount of the carbonized bagasse fiber is 2.2-2.5% of the mass of the natural rubber; Furthermore, silicon dioxide is continuously deposited in at least a portion of the internal pores and the surface of the carbonized bagasse fiber; The deposited amount of silicon dioxide accounts for 25-30% of the total mass of the carbonized bagasse fiber.

6. A method for preparing a rubber sole according to any one of claims 1 to 5, characterized in that: The specific preparation steps include: Carbon coating of flaky inorganic fillers: The flaky inorganic filler and the starch solution are mixed, and an emulsifier is added, and after being stirred and mixed evenly, the mixture is filtered, dried, and after being dispersed, transferred to an inert gas protection state, and heated to carbonize to form an island-shaped carbon coating layer on the surface of the flaky inorganic filler; Preparation of rubber soles: The natural rubber, the flaky inorganic filler with the island-shaped carbon coating layer on the surface, and other additives are mixed and poured into a rubber mixer and mixed evenly to obtain a mixed material; The mixed material is then plasticized in a rubber mixer and extruded into rubber strips; The rubber strip is then transferred into a mold, hot-pressed, vulcanized, and trimmed to obtain a rubber sole.

7. The method for preparing a rubber sole according to claim 6, characterized in that: The other additives include: sulfur, vulcanization accelerator and antioxidant; The vulcanization accelerator is selected from any one of accelerator M, accelerator DM, accelerator MZ, accelerator MTT and accelerator BT; The antioxidant is selected from any one of antioxidant 4010, antioxidant RD, antioxidant MB, antioxidant D, antioxidant AW and antioxidant BLE.

8. The method for preparing a rubber sole according to claim 6, characterized in that: The other additives also include: carbonized bagasse fiber; The preparation steps of the carbonized bagasse fiber include: The sugarcane bagasse is steam exploded, washed, dried, and then heat treated at a temperature of 270-280° C. to obtain heat-treated bagasse; The heat-treated bagasse, ethyl orthosilicate, anhydrous ethanol and oxalic acid are mixed, heated to reflux reaction, and then filtered, washed and dried to obtain a coating precursor; The obtained coated precursor is heated to 780-800° C. under the protection of inert gas and carbonized at high temperature to obtain carbonized bagasse fiber.

Citation Information

Patent Citations

  • Method for producing rubber composition, and rubber composition

    CN105073844A

  • Anti-skid natural rubber material for sneaker soles and preparation method thereof

    CN109181025A

  • Dust ground anti-skid rubber material for shoe soles and preparation method of dust ground anti-skid rubber material

    CN115246959A

  • Heat molding composite sheet material and automotive vehicle interior parts

    JP1998058613A

  • Method for producing natural rubber / inorganic filler masterbatch

    JP2006169292A