High bio-based elastomer cord fabric rubber composition

By using porous three-phase alloys and eutectic solvents in the rubber composition, combined with materials such as rice husk gray-white carbon black, the problems of slow sulfur speed and low thermal conductivity in the rubber are solved, and high bio-based ply rubber is achieved The excellent thermal conductivity and low thermal generation performance meet the high bonding and low thermal generation requirements of tire cord adhesive.

CN118909324AActive Publication Date: 2024-11-08ZHONGCE RUBBER GRP CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411377079.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-30
Publication Date
2024-11-08
Estimated Expiration
2044-09-30

AI Technical Summary

Technical Problem

Bio-based filler rice husk gray white carbon black is slow in rubber composition, resulting in low production efficiency and problems of thermal conductivity and low heat generation. The existing method adds a large amount of vulcanizing agent to cause the rubber to become brittle, heat resistance and physical properties. Got worse.

Method used

Using porous three-phase alloy, prepared from carbon black and natural ore powder through high-temperature jet, combining rice husk gray-white carbon black, silane coupling agent, zinc oxide, anti-aging agent, cobalt salt, methylene donor, methylene acceptor , insoluble sulfur and eutectic solvents form high bio-based elastomer ply rubber compositions, improving thermal conductivity, low heat generation and high fatigue properties.

Benefits of technology

It realizes excellent thermal conductivity, low heat generation and high fatigue properties of high bio-based cord adhesive, meets the requirements of high bonding and low heat generation performance of tire cord adhesive, and solves the slow sulfur speed and poor physical properties of rice husk gray-white carbon black question.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention provides a high bio-based elastomer cord fabric rubber composition, and relates to the technical field of rubber compositions. The rubber composition is mainly prepared by compounding natural rubber, a porous three-phase alloy, rice hull ash white carbon black, a silane coupling agent, zinc oxide, an anti-aging agent, cobalt salt, a methylene donor, a methylene acceptor, insoluble sulfur, an accelerant and a deep eutectic solvent according to a specific proportion. The cord fabric rubber prepared from the high bio-based elastomer cord fabric rubber composition has excellent thermal conductivity, low heat generation and high fatigue performance, and can fully meet the requirements of high adhesion and low heat generation performance of tire cord fabric rubber.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of rubber compositions, in particular to a high-biobased elastomer cord rubber composition. Background Art

[0002] Among the raw materials used in tire production, most of them rely heavily on rubber materials synthesized from fossil resources, which have high carbon emissions and are very unfavorable to the sustainable development of the tire industry.

[0003] In recent years, rice husk ash and silica, as a renewable raw material, have been widely used as a bio-based filler to replace highly dispersed silica in the preparation process of various rubber layers of bio-based tires. This not only reduces the cost of tire production, but also realizes the high added value utilization of biomass resources, greatly reduces the consumption pressure and dependence on petrochemical resources, and is an important direction for the low-carbon and green development of the tire industry in the future.

[0004] The existing tire belt rubber (prepared from the tire cord rubber) requires excellent thermal conductivity, low heat generation, heat-resistant bonding and high fatigue performance. After using the bio-based filler rice husk gray carbon black, the bonding performance of the rubber is significantly improved, and the formed inter-methyl cobalt white bonding system has good steel wire extraction performance. Therefore, using rice husk gray carbon black as a filler to prepare the belt rubber has certain technical advantages.

[0005] However, the bio-based filler rice husk ash white carbon black has a slow vulcanization rate in the rubber composition, resulting in low production efficiency. The conventional method to solve this problem is to add a large amount of vulcanizing agent, but this will cause the rubber to become brittle, and the heat resistance and physical properties will deteriorate. At the same time, the bio-based filler rice husk ash white carbon black also has problems with thermal conductivity and low heat generation.

[0006] Therefore, it is necessary and urgent to research and develop a high-biobased elastomer tire cord rubber composition to alleviate the poor physical properties, slow sulfur rate, low efficiency, thermal conductivity and low heat generation problems of existing bio-based tire cord rubber due to the use of high-biobased rice husk gray carbon black, and then prepare a tire bio-based belt layer rubber with high adhesion and low heat generation performance.

[0007] In view of this, the present invention is proposed. Summary of the invention

[0008] The object of the present invention is to provide a high-biobased elastomer tire cord rubber composition, wherein the tire cord rubber prepared from the rubber composition has excellent thermal conductivity, low heat generation and high fatigue performance, and can fully meet the high adhesion and low heat generation performance requirements of tire cord rubber.

[0009] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted: The present invention provides a porous three-phase alloy, wherein the porous three-phase alloy is mainly prepared by high-temperature jet flow of carbon black and natural ore powder; The content of silicon dioxide in the natural ore powder is 40-60%, and the content of aluminum oxide is 30-40%; The natural mineral powder has a microporous structure and a specific surface area of ​​30-70m 2 / g, pore volume 0.20~0.40cm 3 / g, the number of pores is 100-300 million / g, and the D50 particle size is 0.25-5μm.

[0010] Furthermore, the mass ratio of the carbon black to the natural ore powder is 20~80:80~20; And / or, the carbon black includes at least one of N330, N375, and N326.

[0011] Furthermore, the high temperature jet comprises: The natural ore powder suspension mixed by the jet system is sprayed into the carbon black reaction furnace, and the carbon black reacts with the natural ore powder to form an aluminum-silicon-carbon structure, and then forms an aluminum-silicon-carbon aggregate through aggregation to obtain the porous three-phase alloy; The concentration of the natural ore powder suspension is 15-25wt.%; The injection flow rate of the natural ore powder suspension is 4000-6000 kg / h; The reaction temperature is 1000-1500°C.

[0012] The present invention provides an application of the porous three-phase alloy in the preparation of a high-biobased elastomer cord rubber composition.

[0013] The present invention provides a high-biobased elastomer cord rubber composition, the rubber composition comprising: 100 parts of natural rubber, 5-15 parts of porous three-phase alloy, 30-60 parts of rice husk gray white carbon black, 3-7 parts of silane coupling agent, 8-12 parts of zinc oxide; 3-5 parts of antioxidant; 0.75-1.5 parts of cobalt salt; 3-5 parts of methylene donor; 1-2.5 parts of methylene acceptor; 4-7 parts of insoluble sulfur; 0.8-1.5 parts of accelerator; 0.05-0.5 parts of low eutectic solvent.

[0014] Furthermore, the deep eutectic solvent is mainly prepared from choline chloride and thiourea; The molar ratio of choline chloride to thiourea is (1-3):(3-6), preferably 1:3.

[0015] Furthermore, the specific surface area of ​​the rice husk gray carbon black is 165~240m 2 / g, particle size is 0.8~7.8μm; And / or, the silane coupling agent includes at least one of TESPT, Si75 and Si747; And / or, the accelerator includes at least one of CZ, NS, and DTDM; And / or, the antioxidant includes at least one of 4020, RD, and DTPD; And / or, the methylene donor comprises at least one of melamine resin, melamine formaldehyde resin or hexamethoxymethylmelamine; And / or, the methylene acceptor is at least one of phenolic resin and m-cresol formaldehyde adhesive resin.

[0016] The present invention provides a high-biobased elastomer cord rubber, which is mainly obtained by mixing the high-biobased elastomer cord rubber composition.

[0017] Further, the mixing method comprises the following steps: Natural rubber, porous three-phase alloy, rice husk gray carbon black, silane coupling agent, zinc oxide and antioxidant are mixed according to mass ratio and then kneaded for the first time to obtain rubber mix A; then cobalt salt and methylene acceptor are added to rubber mix A and kneaded for the second time to obtain rubber mix B; Then, the methylene donor, the insoluble sulfur, the accelerator and the low eutectic solvent are added into the rubber compound B for the third mixing to obtain the high bio-based elastomer cord rubber.

[0018] Furthermore, the first mixing includes: mixing at a rotation speed of 45-55 rpm for 30-50 seconds, and then mixing by lifting and pressing the plug for 20-30 seconds until the temperature reaches 140-155° C. for debonding; And / or, the second mixing comprises: mixing at a rotation speed of 25-35 rpm for 30-50 seconds, followed by mixing with the plug lifted and pressed for 20-30 seconds until the temperature reaches 135-145° C. for debonding; And / or, the third mixing includes: mixing at a rotation speed of 25-35 rpm for 30-50 seconds, and then mixing by lifting and pressing the plug for 20-30 seconds to 95-112° C. for debonding.

[0019] Compared with the prior art, the present invention has the following beneficial effects: The porous three-phase alloy provided by the present invention is mainly prepared by high-temperature jetting of carbon black and natural ore powder, wherein the content of silicon dioxide in the natural ore powder is 40-60%, the content of aluminum oxide is 30-40%, and the porous three-phase alloy has a rich microporous structure. After high-temperature jetting treatment, the porous three-phase alloy can be aggregated to form a porous structure alloy material (porous three-phase alloy) of aluminum-silicon-carbon aggregates. The porous three-phase alloy is used in high-biobased elastomer cord rubber, which can effectively improve the thermal conductivity and low heat generation performance of the cord rubber.

[0020] The porous three-phase alloy provided by the present invention can be widely used in the preparation process of a high-biobased elastomer tire cord rubber composition. The prepared tire cord rubber has excellent thermal conductivity, low heat generation and high fatigue performance, and can fully meet the high adhesion and low heat generation performance requirements of tire cord rubber.

[0021] The high bio-based elastomer cord rubber rubber composition provided by the present invention is mainly composed of natural rubber, porous three-phase alloy, rice husk gray carbon black, silane coupling agent, zinc oxide, antioxidant, cobalt salt, methylene donor, methylene acceptor, insoluble sulfur, accelerator, and low eutectic solvent in a specific proportion. In the above-mentioned rubber composition of the present application, rice husk gray carbon black is used to replace the highly dispersible white carbon black, which not only has the characteristics of high bio-based rubber materials, but also has a significant improvement in the adhesive performance of the rubber material; further, the above-mentioned rubber composition effectively solves the problems of thermal conductivity and low heat generation of rice husk gray carbon black by adding porous three-phase alloy; by adding low eutectic solvent, the problems of poor physical properties, slow sulfur rate and low efficiency of high bio-based rice husk gray carbon black in the preparation of tire cord rubber are effectively alleviated. Therefore, the cord rubber rubber prepared by the high bio-based elastomer cord rubber rubber composition of the present application has excellent thermal conductivity, low heat generation and high fatigue performance, which can fully meet the high adhesion and low heat generation performance requirements of tire cord rubber. DETAILED DESCRIPTION

[0022] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0023] According to one aspect of the present invention, a porous three-phase alloy is prepared mainly from carbon black and natural ore powder by high-temperature jet; The content of silicon dioxide in the natural ore powder is 40-60%, and the content of aluminum oxide is 30-40%; The natural mineral powder has a microporous structure and a specific surface area of ​​30-70m 2 / g, pore volume 0.20~0.40cm 3 / g, the number of pores is 100-300 million / g, and the D50 particle size is 0.25-5μm.

[0024] The porous three-phase alloy provided by the present invention is mainly prepared by high-temperature jet from carbon black and natural ore powder, the natural ore powder contains 40-60% silicon dioxide and 30-40% aluminum oxide, and has a rich microporous structure. After high-temperature jet treatment, the porous three-phase alloy can be aggregated to form a porous structure alloy material (porous three-phase alloy) of aluminum-silicon-carbon aggregates. The porous three-phase alloy is used in high-biobased elastomer tire cord rubber, which can effectively improve the thermal conductivity and low heat generation performance of the tire cord rubber, thereby preparing a tire bio-based belt layer rubber with high adhesion and low heat generation performance.

[0025] In a preferred embodiment of the present invention, the mass ratio of the carbon black to the natural ore powder is 20-80:80-20; In a preferred embodiment of the present invention, the carbon black includes at least one of N330, N375, and N326.

[0026] In a preferred embodiment of the present invention, the high temperature jet comprises: The natural ore powder suspension mixed by the jet system is sprayed into the carbon black reaction furnace, and the carbon black reacts with the natural ore powder to form an aluminum-silicon-carbon structure, and then forms an aluminum-silicon-carbon aggregate through aggregation to obtain the porous three-phase alloy; The concentration of the natural ore powder suspension is 15-25wt%; The injection flow rate of the natural ore powder suspension is 4000-6000 kg / h; The reaction temperature is 1000-1500°C.

[0027] According to one aspect of the present invention, the porous three-phase alloy is used in preparing a high bio-based elastomer cord rubber composition.

[0028] The porous three-phase alloy provided by the present invention can be widely used in the preparation process of a high-biobased elastomer cord rubber composition.

[0029] According to one aspect of the present invention, a high bio-based elastomer cord rubber composition comprises: 100 parts of natural rubber, 5-15 parts of porous three-phase alloy, 30-60 parts of rice husk gray white carbon black, 3-7 parts of silane coupling agent, 8-12 parts of zinc oxide; 3-5 parts of antioxidant; 0.75-1.5 parts of cobalt salt; 3-5 parts of methylene donor; 1-2.5 parts of methylene acceptor; 4-7 parts of insoluble sulfur; 0.8-1.5 parts of accelerator; 0.05-0.5 parts of low eutectic solvent.

[0030] The high bio-based elastomer cord rubber rubber composition provided by the present invention is mainly composed of natural rubber, porous three-phase alloy, rice husk gray white carbon black, silane coupling agent, zinc oxide, antioxidant, cobalt salt, methylene donor, methylene acceptor, insoluble sulfur, accelerator, and low eutectic solvent in a specific proportion. In the above-mentioned rubber composition of the present application, rice husk gray white carbon black is used to replace the highly dispersible white carbon black, which not only has the characteristics of high bio-based rubber materials, but also has a significant improvement in the adhesive performance of the rubber material; further, the above-mentioned rubber composition effectively solves the problems of thermal conductivity and low heat generation of rice husk gray white carbon black by adding porous three-phase alloy; by adding low eutectic solvent, the problems of poor physical properties, slow sulfur rate and low efficiency of high bio-based rice husk gray white carbon black in the preparation of tire cord rubber layer are effectively alleviated. Therefore, the cord rubber rubber prepared by the high bio-based elastomer cord rubber rubber composition of the present application has excellent thermal conductivity, low heat generation and high fatigue performance, which can fully meet the high adhesion and low heat generation performance requirements of tire cord rubber.

[0031] At the same time, it should be noted that the methylene donor and the methylene acceptor provide resin cross-linking, thereby enhancing the cross-linking density of the adhesive layer on the surface of the rubber and the steel wire and enhancing the bonding strength between the rubber and the steel wire.

[0032] Zinc oxide forms an oxide film on the surface of the steel wire, increasing the surface roughness of the steel wire and enhancing the bonding between the rubber and the steel wire; secondly, zinc oxide participates in the vulcanization reaction, enhancing the cross-linking of the rubber and further enhancing the bonding between the rubber and the steel wire; Cobalt salts play a vital role in the bonding between rubber and steel wire, which is mainly reflected in the following aspects: 1. The cobalt ions in cobalt salts play a key role in the rubber vulcanization process. It promotes the formation of new material layers between rubber and steel wire, especially metal sulfide layers (such as cuprous sulfide CuxS and zinc sulfide ZnS). These sulfide layers enhance the bonding between rubber and steel wire. Cobalt ions can accelerate the chemical reaction between rubber and steel wire, forming stable chemical bonds, thereby significantly improving the bonding strength. 2. The addition of cobalt salts can accelerate the vulcanization reaction, allowing rubber products to achieve the required physical properties faster.

[0033] It should be noted that the typical but non-limiting preferred embodiments of the addition amount of the porous three-phase alloy are: 5 parts, 6 parts, 7 parts, 8 parts, 9 parts, 10 parts, 11 parts, 12 parts, 13 parts, 14 parts and 15 parts; the typical but non-limiting preferred embodiments of the addition amount of the rice husk gray white carbon black are: 30 parts, 31 parts, 32 parts, 33 parts, 34 parts, 35 parts, 36 parts, 37 parts, 38 parts, 39 parts, 40 parts, 41 parts, 42 parts, 43 parts, 44 parts, 45 parts, 46 parts, 47 parts, 48 ​​parts, 49 parts, 50 parts, 51 parts, 52 parts, 53 parts, 54 parts, 55 parts, 56 parts, 57 parts, 58 parts, 59 parts and 60 parts; the typical but non-limiting preferred embodiments of the addition amount of the above-mentioned silane coupling agent are: 3 parts, 4 parts, 5 parts and 7 parts; the typical but non-limiting preferred embodiments of the addition amount of the above-mentioned zinc oxide are: 8 parts, 9 parts, 10 parts, 11 parts and 12 parts; the addition amount of the above-mentioned antioxidant is: Typical but non-limiting preferred embodiments of the amount of the above cobalt salt are: 0.75 parts, 0.8 parts, 0.9 parts, 1.0 parts, 1.2 parts and 1.5 parts; the typical but non-limiting preferred embodiments of the amount of the above methylene donor are: 3 parts, 4 parts and 5 parts; the typical but non-limiting preferred embodiments of the amount of the above methylene acceptor are: 1 part, 1.5 parts, 1.8 parts , 2.0 parts, 2.3 parts and 2.5 parts; the typical but non-limiting preferred embodiments of the addition amount of the above-mentioned insoluble sulfur are: 4 parts, 5 parts, 6 parts and 7 parts; the typical but non-limiting preferred embodiments of the addition amount of the above-mentioned promoter are: 0.8 parts, 0.9 parts, 1.0 parts, 1.2 parts and 1.5 parts; the typical but non-limiting preferred embodiments of the addition amount of the above-mentioned low eutectic solvent are: 0.05 parts, 0.1 parts, 0.3 parts, 0.4 parts and 0.5 parts.

[0034] In a preferred embodiment of the present invention, the deep eutectic solvent is mainly prepared from choline chloride and thiourea; The molar ratio of choline chloride to thiourea is (1-3):(3-6), preferably 1:3.

[0035] It should be noted that the deep eutectic solvent is prepared from choline chloride and thiourea by the following specific method: In the reaction kettle of the ceramic, stir with a PTFE stirrer, react for 1-4 hours at a water bath reaction temperature of 90-100°C, put into a plastic container after the reaction, and then granulate.

[0036] In a preferred embodiment of the present invention, the specific surface area of ​​the rice husk gray carbon black is 165~240m 2 / g, particle size is 0.8~7.8μm; In a preferred embodiment of the present invention, the silane coupling agent includes at least one of TESPT, Si75 and Si747; In a preferred embodiment of the present invention, the accelerator comprises at least one of CZ, NS, and DTDM; In a preferred embodiment of the present invention, the antioxidant includes at least one of 4020, RD, and DTPD; In a preferred embodiment of the present invention, the methylene donor comprises at least one of melamine resin, melamine formaldehyde resin or hexamethoxymethylmelamine; In a preferred embodiment of the present invention, the methylene acceptor is at least one of a phenolic resin and a m-cresol formaldehyde adhesive resin.

[0037] According to one aspect of the present invention, a high-biobased elastomer cord rubber is provided. The cord rubber is mainly obtained by mixing the above-mentioned high-biobased elastomer cord rubber composition.

[0038] In a preferred embodiment of the present invention, the mixing method comprises the following steps: Natural rubber, porous three-phase alloy, rice husk gray carbon black, silane coupling agent, zinc oxide and antioxidant are mixed according to mass ratio and then kneaded for the first time to obtain rubber mix A; then cobalt salt and methylene acceptor are added to rubber mix A and kneaded for the second time to obtain rubber mix B; Then, the methylene donor, the insoluble sulfur, the accelerator and the low eutectic solvent are added into the rubber compound B for the third mixing to obtain the high bio-based elastomer cord rubber.

[0039] In a preferred embodiment of the present invention, the first mixing comprises: mixing at a rotation speed of 45-55 rpm for 30-50 seconds, followed by mixing with the bolt raised and pressed for 20-30 seconds until the temperature reaches 140-155° C. for debonding; As a preferred embodiment, in the first mixing, the mixing speed is typically but not limited to 40 rpm, 42 rpm, 44 rpm, 46 rpm, 48 rpm, 50 rpm, 52 rpm, 54 rpm and 55 rpm; the mixing time is typically but not limited to 30 s, 32 s, 34 s, 36 s, 38 s, 40 s, 42 s, 44 s, 46 s, 48 ​​s, 50 s; the mixing time of the plug lifting and pressing is typically but not limited to 20 s, 22 s, 24 s, 26 s, 28 s, 30 s, 32 s, 34 s, 36 s, 38 s, 40 s, 42 s, 44 s, 46 s, 48 ​​s, 50 s. s; Typical but non-limiting preferred embodiments of the discharge temperature of the plug-lifting and plug-pressing mixing are: 140°C, 141°C, 142°C, 143°C, 144°C, 145°C, 146°C, 147°C, 148°C, 149°C, 150°C, 151°C, 152°C, 153°C, 154°C, and 155°C.

[0040] In a preferred embodiment of the present invention, the second mixing comprises: mixing at a rotation speed of 25-35 rpm for 30-50 seconds, followed by mixing with the bolt lifting and pressing for 20-30 seconds until the temperature reaches 135-145° C. for debonding; As a preferred embodiment, in the second mixing, the mixing speed is typically but not limited to 25 rpm, 26 rpm, 27 rpm, 28 rpm, 29 rpm, 30 rpm, 31 rpm, 35 rpm, 33 rpm, 34 rpm and 35 rpm; the mixing time is typically but not limited to 30 s, 32 s, 34 s, 36 s, 38 s, 40 s, 42 s, 44 s, 46 s, 48 ​​s, 50 s; the mixing time of the plug lifting and pressing is typically but not limited to 20 s, 22 s, 24 s, 26 s, 28 s, 30 s, 32 s, 34 s, 36 s, 38 s, 40 s, 42 s, 44 s, 46 s, 48 ​​s, 50 s. s; typical but non-limiting preferred embodiments of the discharge temperature of the plug-pressing mixing are: 135°C, 136°C, 137°C, 138°C, 139°C, 140°C, 141°C, 142°C, 143°C, 144°C, and 145°C.

[0041] In a preferred embodiment of the present invention, the third mixing comprises: mixing at a rotation speed of 25-35 rpm for 30-50 seconds, followed by mixing with the plug lifted and pressed for 20-30 seconds to 95-112° C. for debonding.

[0042] As a preferred embodiment, in the third mixing, the mixing speed is typically but not limited to 25 rpm, 26 rpm, 27 rpm, 28 rpm, 29 rpm, 30 rpm, 31 rpm, 35 rpm, 33 rpm, 34 rpm and 35 rpm; the mixing time is typically but not limited to 30 s, 32 s, 34 s, 36 s, 38 s, 40 s, 42 s, 44 s, 46 s, 48 ​​s, 50 s; the mixing time of the plug lifting and pressing is typically but not limited to 20 s, 22 s, 24 s, 26 s, 28 s, 30 s, 32 s, 34 s, 36 s, 38 s, 40 s, 42 s, 44 s, 46 s, 48 ​​s, 50 s. s; typical but non-limiting preferred embodiments of the discharge temperature of the plug-pressing mixing are: 95°C, 96°C, 97°C, 98°C, 99°C, 100°C, 101°C, 102°C, 103°C, 104°C, and 105°C.

[0043] The technical solution of the present invention will be further described below in conjunction with embodiments.

[0044] Example 1 A porous three-phase alloy, wherein the preparation method of the porous three-phase alloy comprises: (1) Raw material preparation: Carbon black N330; Natural ore powder, wherein the content of silicon dioxide in the natural ore powder is 40-60%, and the content of aluminum oxide is 30-40%; the natural ore powder has a microporous structure and a specific surface area of ​​30-70m 2 / g, pore volume 0.20~0.40cm 3 / g, the number of pores is 100-300 million / g, and the D50 particle size is 0.25-5μm.

[0045] (2) High temperature jet: Step 1): The crude oil formula uses low-moisture raw oil (coal tar) with a moisture content of ≤2.0%; the raw oil is mixed with a high-temperature combustion airflow above 1200-1800°C in the reactor section to fully crack the crude oil into primary carbon black particles; Step 2): By using powder jet technology, the porous inorganic material natural ore powder is mixed with process water to obtain a natural ore powder suspension, which is then sprayed into the carbon black reactor; The concentration of the natural ore powder suspension is 20wt.%, and the injection flow rate of the natural ore powder suspension is 5000kg / h; The mass ratio of the carbon black to the natural ore powder is 50:50.

[0046] The specific preparation method is as follows: In the jet system, the natural ore powder and process water are mixed evenly by powder injection technology, and the concentration of the natural ore powder suspension is controlled to be 20wt.%. The natural ore powder suspension is then sprayed into the carbon black reactor by the jet system, and the injection flow rate is 5000kg / h. The mass ratio of carbon black to natural ore powder is controlled, and the temperature in the carbon black reactor is set to 1000℃. Carbon black reacts with natural ore powder to form an aluminum-silicon-carbon structure, which is aggregated to form an aluminum-silicon-carbon aggregate to obtain the porous three-phase alloy.

[0047] The silicon and aluminum atoms of the natural ore powder are chemically combined with the carbon black primary particles at high temperature to form short chain structures of -Si-C-Al-, -Si-OCO-Al- and -Al-O-Si-OC-; the powder jet technology is that the silicon lattice powder is transported to the precisely quantitative embedded double helix through the mechanical arch breaking device, the airflow arch breaking device and the plow blade stirring device at the bottom of the silo in the storage bin, and the silicon lattice powder measured by the weighing system and the precise quantitative spiral enters the mass transfer cavity of the high-speed jet mixer, and is instantly mixed with the jet carrier, i.e., process water. The natural ore powder is forced to be dispersed into the jet carrier during the movement, and is rapidly diffused into a uniform suspension through pressure changes in the diffuser at the tail of the ejector, and is transported to the pressure atomization system; Step 3): Forming three-phase alloy carbon black aggregates through the aggregation of carbon black; Step 4): The carbon black flue gas is collected and separated by the main bag filter. The separated tail gas is used for tail gas furnace heating and boiler power generation. The carbon black is granulated and dried and then stored.

[0048] Embodiment 2~5 A porous three-phase alloy, wherein the preparation method of the porous three-phase alloy comprises: (1) Raw material preparation: same as in Example 1; (2) High temperature jet: Step 1): Same as Example 1; Step 2): In the embodiments 2 to 5, except for the mass ratio of carbon black to natural ore powder, the rest is the same as that of embodiment 1; The mass ratio of the carbon black removal to the natural ore powder is shown in Table 1.

[0049] Table 1:

[0050] Step 3): Same as Example 1; Step 4): Same as Example 1.

[0051] Embodiment 6-8 A high bio-based elastomer cord rubber composition, the composition of the rubber composition is shown in Table 2.

[0052] Table 2:

[0053] The deep eutectic solvent is prepared from choline chloride and thiourea, and the molar ratio of choline chloride to thiourea is 2:4; The specific method includes: stirring in a ceramic reactor with a PTFE stirrer, reacting for 1-4 hours at a water bath reaction temperature of 90-100° C., placing in a plastic container after the reaction, and then granulating.

[0054] The tire cord rubber composition is mixed to obtain the tire cord rubber, and the specific method includes: Stage 1 masterbatch: start the internal mixer, set the speed to 50 rpm, first add natural rubber, porous three-phase alloy, rice husk gray carbon black, silane coupling agent, zinc oxide and antioxidant, mix for 40 seconds, remove the plug and press the plug to mix for 25 seconds, remove the plug and press the plug to mix until the temperature reaches 150°C to discharge the glue, and obtain masterbatch 1; Second stage masterbatch: start the internal mixer, set the speed to 30 rpm, first add masterbatch 1, cobalt salt and methylene acceptor, mix for 40 seconds, remove the plug and mix for 25 seconds, remove the plug and mix until the temperature reaches 140℃ to discharge the glue, and obtain masterbatch 2; Vulcanization: Start the internal mixer, set the speed to 30 rpm, first add masterbatch 2, methylene donor, insoluble sulfur, accelerator and low eutectic solvent, mix for 40 seconds, remove the plug and mix for 25 seconds, remove the plug and mix until 100°C to discharge the rubber, and obtain the cord rubber.

[0055] Example 9 This embodiment is the same as Embodiment 6 except that the porous three-phase alloy prepared in Embodiment 2 is used to replace the porous three-phase alloy prepared in Embodiment 1.

[0056] Example 10 This embodiment is the same as Embodiment 6 except that the porous three-phase alloy prepared in Embodiment 3 is used to replace the porous three-phase alloy prepared in Embodiment 1.

[0057] Embodiment 11 This embodiment is the same as Embodiment 6 except that the porous three-phase alloy prepared in Embodiment 4 is used to replace the porous three-phase alloy prepared in Embodiment 1.

[0058] Example 12 This embodiment is the same as Embodiment 6 except that the porous three-phase alloy prepared in Embodiment 5 is used to replace the porous three-phase alloy prepared in Embodiment 1.

[0059] Test Example 1 In order to show that the high bio-based elastomer cord rubber composition of the present application can effectively alleviate the problems of poor physical properties, slow sulfurization rate and low efficiency caused by the use of high bio-based rice husk gray carbon black in existing bio-based tires, as well as the problems of thermal conductivity and low heat generation of bio-based filler rice husk gray carbon black, the high bio-based elastomer cord rubber composition prepared in Examples 6 to 12 is now used for testing, and the specific results are shown in Tables 3 and 4 below.

[0060] Table 3:

[0061] Note: In Table 3, when the vulcanization test condition is 140℃*60min, MH is the maximum torque; ML is the minimum torque; Ts2 is the time corresponding to (minimum torque + 0.2Nm); T10 is the time corresponding to (minimum torque + (maximum torque - minimum torque) × 0.1), also known as the scorch time; T30 is the time corresponding to (minimum torque + (maximum torque - minimum torque) × 0.3); T60 is the time corresponding to (minimum torque + (maximum torque - minimum torque) × 0.6); T90 is the time corresponding to (minimum torque + (maximum torque - minimum torque) × 0.9), also known as the positive vulcanization time. Rev97 is the return vulcanization time; M300 is the 300% tensile strength of the vulcanized rubber; TB is the tensile strength of the vulcanized rubber; tanδ / 60℃ is the loss factor at 60℃.

[0062] It should be noted that the meanings of the test items in the test result tables of the following Test Examples 1 to 4 are the same as those in Table 3.

[0063] Table 4:

[0064] It can be seen from Tables 3 and 4 above that the tire cord rubber compositions prepared in Examples 6 to 10 (porous three-phase alloys prepared with a carbon black to natural ore powder ratio in the range of 20 to 80:80 to 20) have better thermal conductivity and low heat generation effects.

[0065] However, the mass ratio of carbon black to natural ore powder in the porous three-phase alloy of the cord rubber composition of Examples 11 and 12 is not within the range of 20-80:80:20, and the reinforcement effect of the prepared rubber composition is deteriorated. It can be seen from Example 11 that TB is reduced and the heat generation is increased compared with Example 6.

[0066] Embodiment 13 This embodiment is the same as Embodiment 6 except that the molar ratio of choline chloride to thiourea in the deep eutectic solvent is 1:3.

[0067] Embodiment 14 This embodiment is the same as Embodiment 6 except that the molar ratio of choline chloride to thiourea in the deep eutectic solvent is 3:6.

[0068] Embodiment 15 This embodiment is the same as Embodiment 6 except that the molar ratio of choline chloride to thiourea in the deep eutectic solvent is 4:3.

[0069] Example 16 This embodiment is the same as Embodiment 6 except that the molar ratio of choline chloride to thiourea in the deep eutectic solvent is 5:3.

[0070] Embodiment 17 This embodiment is the same as Embodiment 6 except that the molar ratio of choline chloride to thiourea in the deep eutectic solvent is 1:8.

[0071] Test Example 2 In order to show that the raw material composition of the deep eutectic solvent has a significant effect on the performance of the tire cord rubber composition of the present application, the tire cord rubber composition prepared in Examples 13 to 17 is used for testing, and the specific results are shown in Table 5 below.

[0072] Table 5:

[0073] It can be seen from Table 5 above that the technical effects of the tire cord rubber composition prepared in Examples 13 and 14 are almost the same as those in Example 6, and the technical effects of the tire cord rubber composition of the present application can be achieved.

[0074] However, the composition of the low eutectic solvent in the tire cord rubber composition of Examples 15 to 17 is not within the range of "the molar ratio of choline chloride to thiourea is (1 to 3): (3 to 6)" in the present application, and the effect of improving the sulfur rate of the tire cord rubber composition is not obvious. In other words, only the low eutectic solvent prepared within the range of "the molar ratio of choline chloride to thiourea is (1 to 3): (3 to 6)" in the present application can effectively alleviate the problems of poor physical properties, slow sulfur rate and low efficiency of high bio-based rice husk gray white carbon black in the preparation of tire cord rubber layer.

[0075] Embodiment 18 This embodiment is the same as that of Example 1 except that the mixing process parameters of the tire cord rubber composition are different from those of Example 1; The mixing method of the tire cord rubber composition comprises: Stage 1 masterbatch: start the internal mixer and set the speed to 45 rpm. First add natural rubber, porous three-phase alloy, rice husk gray carbon black, silane coupling agent, zinc oxide and antioxidant, mix for 50 seconds, remove the plug and press the plug to mix for 20 seconds, remove the plug and press the plug to mix until the temperature reaches 140°C to discharge the glue, and obtain masterbatch 1; Second stage masterbatch: start the internal mixer, set the speed to 25 rpm, first add masterbatch 1, cobalt salt and methylene acceptor, mix for 50 seconds, remove the plug and press the plug to mix for 20 seconds, remove the plug and press the plug to mix until the temperature reaches 145°C to discharge the glue, and obtain masterbatch 2; Vulcanization: Start the internal mixer, set the speed to 25 rpm, first add masterbatch 2, methylene donor, insoluble sulfur, accelerator and low eutectic solvent, mix for 50 seconds, remove the plug and mix for 20 seconds, remove the plug and mix until the temperature is 95°C to discharge the glue, and obtain the cord rubber.

[0076] Embodiment 19 This embodiment is the same as that of Example 1 except that the mixing process parameters of the tire cord rubber composition are different from those of Example 1; The mixing method of the tire cord rubber composition comprises: Stage 1 masterbatch: start the internal mixer and set the speed to 55 rpm. First add natural rubber, porous three-phase alloy, rice husk gray carbon black, silane coupling agent, zinc oxide and antioxidant, mix for 30 seconds, lift the plug and press the plug to mix for 30 seconds, lift the plug and press the plug to mix until the temperature reaches 155°C to discharge the rubber, and obtain masterbatch 1; Second stage masterbatch: start the internal mixer, set the speed to 35 rpm, first add masterbatch 1, cobalt salt and methylene acceptor, mix for 30 seconds, lift the plug and press the plug to mix for 30 seconds, lift the plug and press the plug to mix until the temperature reaches 135°C to discharge the glue, and obtain masterbatch 2; Vulcanization: Start the internal mixer, set the speed to 35 rpm, first add masterbatch 2, methylene donor, insoluble sulfur, accelerator and low eutectic solvent, mix for 30 seconds, lift the bolt and press the bolt to mix for 30 seconds, lift the bolt and press the bolt to mix until the glue is discharged at 112°C to obtain the cord rubber.

[0077] Test Example 3 In order to show that the mixing method of the tire cord rubber composition of the present application has a significant effect on the performance of the tire cord rubber composition of the present application, the tire cord rubber prepared in Examples 18 and 19 is used for testing, and the specific results are shown in Table 6 below.

[0078] Table 6:

[0079] It can be seen from Table 6 above that the heat conduction problem can be effectively solved under the mixing method of the present application, and the heat generation is also slightly reduced.

[0080] Comparative Examples 1 to 3 A high bio-based elastomer cord rubber composition, the composition of the rubber composition is shown in Table 7: Table 7:

[0081] The mixing methods of the tire cord rubber compositions of the above comparative examples are carried out in accordance with the method of Example 2.

[0082] Comparative Example 4 This comparative example is the same as Example 2 except that it does not contain the "porous three-phase alloy".

[0083] Comparative Example 5 This comparative example is the same as Example 2 except that it does not contain a “deep eutectic solvent”.

[0084] Comparative Example 6 This comparative example is the same as Example 2 except that it does not contain "methylene donor and methylene acceptor".

[0085] Comparative Example 7 This comparative example is the same as Example 2 except that an equal amount of rice husk ash carbon black is replaced by carbon black N375.

[0086] Test Example 4 In order to show that the high bio-based elastomer cord rubber composition of the present application can effectively alleviate the problems of poor physical properties, slow sulfurization rate and low efficiency caused by the use of high bio-based rice husk gray carbon black in existing bio-based tires, as well as the problems of thermal conductivity and low heat generation of bio-based filler rice husk gray carbon black, the cord rubber prepared in Comparative Examples 1 to 7 is now used for testing, and the specific results are shown in Tables 8 and 9 below: Table 8:

[0087] Table 9:

[0088] From Tables 8 and 9 above, it can be seen from Comparative Examples 1 to 3 that the sulfur rate of rice husk gray carbon black is slow, the thermal conductivity is low, and the heat generation is low. The use of porous three-phase alloy can greatly improve the thermal conductivity; the adhesion of rice husk gray carbon black is improved; by comparing Comparative Example 2 with Examples 2 to 6, it can be seen that the sulfur rate can be well adjusted by adding a low eutectic solvent, and MH is basically unchanged. Compared with Examples 2 to 6, the implementation method of Comparative Example 4 that does not include "porous three-phase alloy" has significantly decreased thermal conductivity, decreased elongation, and decreased MH; Compared with Examples 2 to 6, the implementation method of Comparative Example 5 that does not include "low eutectic solvent" has significantly slowed down the sulfur rate; Compared with Examples 2 to 6, the implementation method of Comparative Example 6 that does not include "methylene donor, methylene acceptor" has decreased MH and greatly decreased bonding strength; Compared with Examples 2 to 6, the implementation method of Comparative Example 7 except replacing the rice husk gray carbon black with carbon black N375 in equal amounts has increased MH and greatly increased heat generation.

[0089] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A high bio-based elastomer cord rubber composition, characterized in that: The rubber composition comprises, by weight: 100 parts of natural rubber, 5-15 parts of porous three-phase alloy, 30-60 parts of rice husk gray white carbon black, 3-7 parts of silane coupling agent, 8-12 parts of zinc oxide; 3-5 parts of antioxidant; 0.75-1.5 parts of cobalt salt; 3-5 parts of methylene donor; 1-2.5 parts of methylene acceptor; 4-7 parts of insoluble sulfur; 0.8-1.5 parts of accelerator; 0.05-0.5 parts of low eutectic solvent; The porous three-phase alloy is mainly prepared by high-temperature jetting of carbon black and natural ore powder; The content of silicon dioxide in the natural ore powder is 40-60%, and the content of aluminum oxide is 30-40%; the natural ore powder has a microporous structure and a specific surface area of ​​30-70m 2 / g, pore volume 0.20~0.40cm 3 / g, the number of pores is 100-300 million / g, and the D50 particle size is 0.25-5μm.

2. The high bio-based elastomer cord rubber composition according to claim 1, characterized in that: The mass ratio of the carbon black to the natural ore powder in the porous three-phase alloy is 20-80:80-20.

3. The high bio-based elastomer cord rubber composition according to claim 1, characterized in that: The carbon black includes at least one of N330, N375 and N326.

4. The high bio-based elastomer cord rubber composition according to claim 1, characterized in that: The high temperature jet comprises: The natural ore powder suspension mixed by the jet system is sprayed into the carbon black reaction furnace, and the carbon black reacts with the natural ore powder to form an aluminum-silicon-carbon structure, and then forms an aluminum-silicon-carbon aggregate through aggregation to obtain the porous three-phase alloy; The concentration of the natural ore powder suspension is 15-25wt%; The injection flow rate of the natural ore powder suspension is 4000-6000 kg / h; The reaction temperature is 1000-1500°C.

5. The high bio-based elastomer cord rubber composition according to claim 1, characterized in that: The deep eutectic solvent is mainly prepared from choline chloride and thiourea; The molar ratio of choline chloride to thiourea is (1-3): (3-6).

6. The high bio-based elastomer cord rubber composition according to claim 1, characterized in that: The specific surface area of ​​the rice husk gray carbon black is 165~240m 2 / g, particle size is 0.8~7.8μm; And / or, the silane coupling agent includes at least one of TESPT, Si75 and Si747; And / or, the accelerator includes at least one of CZ, NS, and DTDM; And / or, the antioxidant includes at least one of 4020, RD, and DTPD; And / or, the methylene donor comprises at least one of melamine resin, melamine formaldehyde resin or hexamethoxymethylmelamine; And / or, the methylene acceptor is at least one of a phenolic resin and a m-cresol formaldehyde adhesive resin.

7. A high bio-based elastomer cord rubber, characterized in that: The tire cord rubber is mainly obtained by mixing the high bio-based elastomer tire cord rubber composition according to any one of claims 1 to 6.

8. The high bio-based elastomer cord rubber according to claim 7, characterized in that: The mixing method comprises the following steps: Natural rubber, porous three-phase alloy, rice husk gray carbon black, silane coupling agent, zinc oxide and antioxidant are mixed according to mass ratio and then kneaded for the first time to obtain rubber mix A; then cobalt salt and methylene acceptor are added to rubber mix A and kneaded for the second time to obtain rubber mix B; Then, the methylene donor, the insoluble sulfur, the accelerator and the low eutectic solvent are added into the rubber compound B for the third mixing to obtain the high bio-based elastomer cord rubber.

9. The high bio-based elastomer cord rubber according to claim 8, characterized in that: The first mixing includes: mixing at a rotation speed of 45-55 rpm for 30-50 seconds, and then mixing with the plug lifting and pressing for 20-30 seconds until the temperature reaches 140-155° C. for debonding; And / or, the second mixing comprises: mixing at a rotation speed of 25-35 rpm for 30-50 seconds, and then mixing with the plug lifting and pressing for 20-30 seconds until the temperature reaches 135-145° C. for debonding; And / or, the third mixing includes: mixing at a rotation speed of 25-35 rpm for 30-50 seconds, and then mixing by lifting and pressing the plug for 20-30 seconds to 95-112° C. for debonding.

Citation Information

Patent Citations

  • Antistatic oxidation-resistant thermal barrier coating and preparation method thereof

    CN105112847A

  • Low-heat-generation puncture-resistant rubber composition for engineering radial tire and preparation method thereof

    CN111499933A

  • PBAT composite material and preparation method and application thereof

    CN113388238A

  • High-performance cord fabric rubber for tires and preparation method of high-performance cord fabric rubber

    CN114381045A

  • Low-heat tire wire cord fabric rubber composition and preparation method thereof

    CN117603508A