Three-dimensional impact-resistant protective material as well as preparation method and application thereof
Through the construction of dual continuous IPN composite materials, combined with IHP materials and EVA foaming materials, the contradiction between impact protection materials in external force sensitivity and energy absorption efficiency is solved, and the high-efficiency energy absorption and self-healing characteristics are achieved, and the material is improved Fatigue resistance and shape stability.
Patent Information
- Application Number
- CN202410956615.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-17
AI Technical Summary
There is a contradiction between external force sensitivity and energy absorption efficiency in existing impact protection materials, and their fatigue resistance and shape stability are poor, making it difficult to achieve ideal intelligent protection functions.
Using a dual continuous IPN composite material, the mesh polymer is constructed by mixing the IHP material containing silicon boron with polysiloxane, branched MQ resin or thermoplastic elastomer at 60°C, and the EVA foaming material is used as a carrier. , through blending foaming, the material has external force sensitivity and self-healing characteristics.
It achieves the improvement of high external force sensitivity and energy absorption efficiency, and at the same time improves the fatigue resistance and shape stability of the material, avoids the use of high-temperature catalysts and the occurrence of side reactions, and enhances the forming performance of the material.
Smart Images

Figure CN118909342A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of composite materials, and in particular relates to a three-dimensional impact-resistant protective material, a preparation method and application thereof. Background Art
[0002] Impact-resistant protective materials use the response characteristics of materials to external forces to achieve intelligent protection of receptors. They can ensure that the materials remain soft and comfortable under normal conditions, but once they are subjected to external force impact, they quickly harden, absorb and dissipate impact energy, and provide effective protection for the receptors. Therefore, they have broad application prospects in sports protection, military and police protection, and material packaging. Traditional impact-resistant protective materials include inorganic rigid materials (such as cement, metal materials, etc.), high-strength polymer fibers (such as ultra-high molecular weight polyethylene, Kevlar fibers, etc.), porous foam materials, and damping materials (such as polyurethane, cross-linked rubber, etc.), which have been widely used in the field of protection. Although porous foam materials and shock-absorbing damping materials have good energy absorption efficiency, these materials have poor fatigue resistance, low energy absorption efficiency, and lack of intelligent functions, which make it impossible to achieve the ideal intelligent protection function we expect. Some materials with a certain degree of external force sensitivity mainly transmit the energy generated by external forces when they are in a hardened state, and the energy absorption efficiency is low.
[0003] In response to the above problems, some people have designed new intelligent protection systems, among which the shear thickening fluid (STF) system of the US Army Laboratory and the DEFLXION series of Dowcorning in the United States are more representative intelligent protection products. Since the US Army Laboratory first launched the "liquid armor" made of shear thickening fluid technology in 2005, the ideal intelligent protection material is gradually becoming a reality. STF technology uses inorganic nanoparticles (such as silica, calcium carbonate, etc.) dispersed in the fluid phase (such as polyethylene glycol) to aggregate under the shear action of external force, resulting in a unique fluid behavior in which the viscosity of the fluid system suddenly increases. Combined with the wetting effect of the mobile phase in the STF system on the fiber material, the STF system is compounded inside the fiber material. Then, the soft-hard transformation of the composite fiber material in the natural state and the external force impact state is realized (the change range of the material modulus can reach 2-3 orders of magnitude), and at the same time, the aggregation and dispersion process of a large number of inorganic nanoparticles in the system is used to absorb most of the impact energy, and finally complete the effective protection of the external force receptor. However, due to the limitations of the solvation effect of the fluid on the fiber material in the STF system and the easy leakage of the fluid system, the STF system cannot be widely used in all fiber material fields. Dow Corning of the United States uses the swelling characteristics of silicon-boron copolymers to prepare swelling materials, and composites them with fabrics of different structures to develop a series of sports functional protective materials DEFLXION product series. This technology uses functional silane and boric acid to condense under catalyst and high temperature conditions (150-200℃). Swelling materials have a certain external force sensitivity under the action of external forces. The elastic modulus ratio (G'max / G'min) of the material at 0.1Hz and 400Hz shear frequencies in rheological tests is used as a reference standard to characterize the external force sensitivity of the material, which can reach about 10-500 times. As a well-known intelligent protection product in the international market, the emergence of swelling materials has attracted the attention of many people, but the related basic scientific research on principles and the innovative development of subsequent products are relatively lagging behind. While showing good technical characteristics and application potential, swelling materials also have obvious technical defects. For example: 1) The material preparation process is harsh, requiring the presence of toxic and harmful catalysts and a high reaction temperature (150-200°C); 2) Under high temperature conditions (100-150°C), boric acid is easily converted into metaboric acid and pyroboric acid, which will lead to the appearance of many side reaction products. The reaction products at lower temperatures have lower molecular weights, poor mechanical strength and easy hydrolysis, which limits the practical application of the products; 3) Material weather resistance issues. Under low temperature conditions (<-20°C), the material becomes more brittle and its performance decreases; 4) The swelling material will break under the impact of a large external force and cannot be actively repaired, which makes the material have poor fatigue resistance during application. In its actual application process, in order to improve the molding and processing performance of the swelling material, a large amount of inorganic materials and third components are added, which further reduces its fatigue resistance.
[0004] In summary, the current protective materials have the following problems in the research process: 1. It is impossible to achieve the joint improvement of external force sensitivity and energy absorption efficiency. The realization of intelligent material protection mainly depends on the ability of the material to change its own strength under normal and stress conditions, as well as the absorption efficiency of impact energy. In the existing system, porous foam materials and shock-absorbing damping materials have good energy absorption efficiency, but these materials themselves do not have the characteristics of intelligent response to external forces. Some materials with a certain degree of external force sensitivity mainly transmit the energy generated by external forces when they are in a hardened state, and the energy absorption efficiency is relatively low; 2. The contradiction between material fatigue resistance, energy absorption efficiency and shape stability; among the many properties of protective materials, high external force sensitivity requires that the material preferably has a dynamic cross-linking state, so the mechanical strength of the material is relatively low, and the ability to maintain its own shape is weak. The improvement of the material's energy absorption efficiency requires the material to have obvious viscosity characteristics, which also makes the material low in strength and poor in formability. For most protective materials, the damage caused by impact is difficult to repair actively, so the fatigue resistance of the material is very poor. The use of dynamic cross-linking structures or self-adhesion of rubber materials can achieve self-repair of damaged materials under external impact, thereby improving the fatigue resistance of the material. However, it will also cause the material to have poor formability and cannot be used freely as a bulk material.
[0005] Therefore, there is an urgent need to prepare a three-dimensional impact-resistant protective material with high yield, intelligent response to external forces, high energy absorption efficiency, good material fatigue resistance and shape stability. Summary of the invention
[0006] In view of the above-mentioned shortcomings of the prior art, the purpose of the present application is to provide a three-dimensional impact-resistant protective material and a preparation method thereof with high productivity, intelligent response to external forces, high energy absorption efficiency, good material fatigue resistance and shape stability.
[0007] In order to achieve the above-mentioned object and other related objects, the present application provides a three-dimensional impact-resistant protective material, characterized in that it is made from raw materials containing the following components in parts by weight:
[0008]
[0009]
[0010] The bicontinuous IPN composite material is a network polymer constructed by mixing and heating at 60° C. for 2 to 3 hours with IHP material containing silicon and boron as the first continuous phase and one or more of polysiloxane, branched MQ resin or thermoplastic elastomer as the second continuous phase.
[0011] More preferably, the three-dimensional impact-resistant protective material is characterized in that it is made from raw materials containing the following components in parts by weight:
[0012]
[0013] The bicontinuous IPN composite material is a network polymer constructed by mixing and reacting at 60° C. for 2 to 3 hours with a silicon-boron-containing IHP material as the first continuous phase and one or more of polysiloxane, branched MQ resin or thermoplastic elastomer as the second continuous phase.
[0014] Preferably, the structure of the IHP material is shown in formula (I):
[0015]
[0016] Among them, m is 10 to 100 and n is 10 to 100.
[0017] Preferably, the vulcanizing agent is BIBP; the coupling agent is KH-570; and the foaming agent is AC3000h.
[0018] The present application also provides a method for preparing a three-dimensional impact-resistant protective material, which is characterized by comprising the following steps:
[0019] Step 1: Preparation of IHP materials:
[0020] (1) reacting polysiloxane with a boron-containing crosslinking agent at 50 to 90° C. for 3 to 6 hours to obtain a crosslinked product; the mass ratio of the polysiloxane to the boron-containing crosslinking agent is 10 to 100:1;
[0021] (2) mixing the cross-linked product with a chain extender, reacting at 60 to 9° C. for 2 to 6 hours to obtain an IHP material precursor having a network structure; the mass ratio of the polysiloxane to the chain extender is 20 to 100:1;
[0022] (3) thermally treating and / or mechanically treating the IHP material precursor to ultimately prepare an IHP material having both external force sensitivity and self-healing properties;
[0023] Step 2, constructing a bicontinuous IPN composite material: using the IHP material as the first continuous phase, and using one or more of polysiloxane, branched MQ resin or thermoplastic elastomer as the second continuous phase, mixing and heating at 60° C. for 2 to 3 hours to construct a bicontinuous IPN composite material;
[0024] Step 3, preparing a three-dimensional impact protection material: using an IHP material and / or a bicontinuous IPN composite material as a main body and an EVA foam material as a carrier, dispersing the IHP material and / or the bicontinuous IPN composite material inside the EVA by blending and foaming to obtain a three-dimensional impact protection material; wherein the mass ratio of the dispersed main body to the EVA foam material is 5-30:60-110;
[0025] Preferably, in step 1(1), the polysiloxane is one or more of bishydroxy-terminated polydimethylsiloxane, bisamino-terminated polydimethylsiloxane, vinyl-terminated hydroxyl-terminated polydimethylsiloxane, vinyl-terminated amino-polydimethylsiloxane, hydrogen-terminated hydroxyl-terminated polydimethylsiloxane, hydrogen-terminated amino-polydimethylsiloxane and vinyl-terminated hydrogen-terminated polydimethylsiloxane.
[0026] More preferably, in step 1(1), the polysiloxane is dihydroxy-terminated polydimethylsiloxane with a weight average molecular weight of 1,000 to 20,000 and a viscosity of 50 to 100 cps.
[0027] Preferably, in step 1(1), the boron-containing cross-linking agent is one or more of borates, boric acid compounds, boric esters and trimethoxyboroxane.
[0028] More preferably, in step (1), the boron-containing cross-linking agent is trimethoxyboroxane as shown in Figure (II).
[0029] Preferably, in step (1), the mass ratio of the dihydroxy-terminated polydimethylsiloxane to the trimethoxyboroxane is 10 to 100:1.
[0030] More preferably, in step (1), the mass ratio of the dihydroxy-terminated polydimethylsiloxane to the trimethoxyboroxane is 40:1.
[0031] Preferably, the chain extender is a diisocyanate or a polyisocyanate.
[0032] More preferably, the chain extender is a diisocyanate represented by formula (VI).
[0033] Preferably, the mass ratio of the dihydroxy-terminated polydimethylsiloxane in step (1) to the diisocyanate in step (2) is 5-10:0.1-0.25.
[0034] More preferably, the mass ratio of the dihydroxy-terminated polydimethylsiloxane in step (1) to the chain extender in step (2) is 5:0.2.
[0035] Since trimethoxyboroxane is a compound that is easily decomposed in water and sensitive to air, it first decomposes into methanol and trimethyl borate shown in formula (III) during the reaction. Trimethyl borate reacts with dihydroxy-terminated polydimethylsiloxane shown in formula (IV) at a temperature below 90°C for 3 to 6 hours to obtain a cross-linked product shown in formula (V). The entire reaction process is carried out at a temperature not higher than 90°C without the addition of a catalyst. The side reaction of boric acid being converted into pyroboric acid and metaboric acid caused by high temperature can be completely avoided, reducing or avoiding the appearance of by-products. At the same time, due to the high reactivity of isocyanate, the product can be guaranteed to have a high molecular weight.
[0036] Preferably, in step (3), tetraisopropyl titanate represented by formula (VIII) is used as a hydrolysis modifier to modify the IHP material precursor represented by formula (VII); the mass ratio of the dihydroxy-terminated polydimethylsiloxane in step (1) to the tetraisopropyl titanate in step (3) is 5 to 10:0.1 to 0.5.
[0037] More preferably, the mass ratio of the dihydroxy-terminated polydimethylsiloxane in step (1) to the tetraisopropyl titanate in step (3) is 200:1.
[0038] Preferably, the second continuous phase is polysiloxane with a weight average molecular weight of 2,000 to 10,000.
[0039] Preferably, in step 2, the mass ratio of the first continuous phase to the second continuous phase is 1:0.5-1.
[0040] More preferably, in step 2, the mass ratio of the first continuous phase to the second continuous phase is 1:0.5-0.8.
[0041] More preferably, in step 2, the mass ratio of the first continuous phase to the second continuous phase is 1:0.6.
[0042] In step 3 of the present invention, the three-dimensional impact protection material is prepared according to the following method, including:
[0043] Weigh 5 to 30 parts of bicontinuous IPN composite material, 60 to 110 parts of EVA resin, 5 to 30 parts of polyurethane black and white material, 0.5 to 5 parts of vulcanizing agent, 5 to 30 parts of coupling agent, and 0.5 to 2 parts of foaming agent by weight, and mix them to prepare EVA / IHP blended material; the mixing or twin-screw extrusion temperature is 90 to 120°C;
[0044] The EVA / IHP blended material is subjected to mold compression foaming to prepare a three-dimensional impact protection foam material; the molding pressure is 18 MPa; and the molding time is 6 to 15 minutes.
[0045] Preferably, the EVA resin is an ethylene-vinyl acetate copolymer, the vinyl acetate content in the EVA resin is 15-22%, and the molecular weight is 30,000-80,000.
[0046] Preferably, the mass ratio of the bicontinuous IPN composite material to the EVA resin is 10-35:90-110.
[0047] More preferably, the mass ratio of the bicontinuous IPN composite material to the EVA resin is 25:100.
[0048] Preferably, the mass ratio of the polyurethane black and white material to the EVA resin is 10-15:90-100.
[0049] More preferably, the mass ratio of the polyurethane black and white material to the EVA resin is 10:100.
[0050] Preferably, the EVA / IHP blend material in step 3 is prepared by the following method: 25 parts of bicontinuous INP composite materials, 100 parts of EVA resin (ethylene-vinyl acetate copolymer, vinyl acetate content 15-22%, molecular weight 30000-80000), 10 parts of polyurethane black and white materials, 1 part of vulcanizing agent, 6 parts of coupling agent, and 0.8 parts of foaming agent are weighed by weight to prepare EVA / IHP blend material; the mixing or twin-screw extrusion temperature is 90-120°C.
[0051] The present application also provides an application of the three-dimensional impact-resistant protective material or the three-dimensional impact-resistant protective material prepared by the preparation method of the three-dimensional impact-resistant protective material in sports protective materials. The application includes use as the lining of helmets and / or sports protective articles such as knee pads, elbow pads, yoga mats, etc., or together with fabrics to form sports protective textiles, etc.
[0052] The beneficial effects of this application are:
[0053] 1. The entire reaction process of the three-dimensional impact-resistant protective material prepared in this application is carried out at a temperature not higher than 90°C, without the addition of a catalyst. The side reaction of boric acid being converted into pyroboric acid and metaboric acid caused by high temperature can be completely avoided, and the appearance of by-products can be reduced or avoided. At the same time, due to the high reactivity of isocyanate, the product can be guaranteed to have a high molecular weight.
[0054] 2. This application constructs a new type of impact-hardening polymer (IHP material) based on the comprehensive STF technology and the technical characteristics of the expansion material. The material has excellent impact hardening and self-healing properties, showing good development prospects.
[0055] 3. The dual-continuous IPN composite material prepared with IHP material as the main body, the composite material is kept in the environment of low temperature -23℃±2℃ and high temperature ﹢50℃±5℃ for 4 hours, the impact force value is 3J, and the sensing impact force is ≤6KN; it is kept in the environment of normal temperature 23℃±2℃ and low temperature -50°±2° for 4 hours, and then taken out and folded up and down 10,000 times. There is no delamination, deformation or bulging, fracture and damage on the appearance, realizing the positive synergistic regulation mechanism of the various properties of the two continuous phases, while ensuring that the material has high external force sensitivity and self-healing ability, and can also improve the shape maintenance ability of the material;
[0056] 4. The three-dimensional impact-resistant protective material prepared from the bicontinuous IPN composite material has good formability, and the impact test transmission force value is ≤35kN (impact energy is 50J). The damage caused by the impact can be quickly and actively repaired, achieving a joint improvement in external force sensitivity and energy absorption efficiency, solving the contradiction between material fatigue resistance, energy absorption efficiency and shape stability, and preparing a three-dimensional impact-resistant protective material. BRIEF DESCRIPTION OF THE DRAWINGS
[0057] Figure 1 Shown is the synthetic route for preparing the IHP material in Example 1.
[0058] Figure 2 Shown is the SEM image of the IHP material prepared in Example 1.
[0059] Figure 3 Shown is the rheological spectrum of the IHP material prepared in Example 1.
[0060] Figure 4 Shown is the SEM image of the bicontinuous IPN composite material prepared in Example 11.
[0061] Figure 5 Shown is the XRD spectrum of the bicontinuous IPN composite material prepared in Example 11.
[0062] Figure 6 Shown is one of the SEM images of the three-dimensional impact-resistant protective material prepared in Example 16.
[0063] Figure 7 The second SEM image shows the three-dimensional impact-resistant protective material prepared in Example 16.
[0064] Figure 8 The impact performance of the impact-resistant protective foam material prepared in Example 18 is shown. DETAILED DESCRIPTION
[0065] The following describes the implementation of the present application through specific examples, and those skilled in the art can easily understand other advantages and effects of the present application from the contents disclosed in this specification. The present application can also be implemented or applied through other different specific implementations, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present application.
[0066] It should be noted that the process equipment or devices not specifically specified in the following embodiments are all conventional equipment or devices in the art.
[0067] In addition, it should be understood that one or more method steps mentioned in this application do not exclude the existence of other method steps before or after the combination step or the insertion of other method steps between these explicitly mentioned steps, unless otherwise specified; it should also be understood that the combination connection relationship between one or more devices / apparatuses mentioned in this application does not exclude the existence of other devices / apparatuses before or after the combination device / apparatus or the insertion of other devices / apparatuses between these two explicitly mentioned devices / apparatuses, unless otherwise specified. Moreover, unless otherwise specified, the numbering of each method step is only a convenient tool for identifying each method step, and is not intended to limit the order of arrangement of each method step or the scope of implementation of this application. Changes or adjustments in their relative relationships shall also be regarded as the scope of implementation of this application without substantial changes in the technical content.
[0068] In the following embodiments of the present application, the main testing standards and equipment information are as follows: Reference standard GA420-2021 "Police Anti-Riot Clothing" is used to test the impact protection performance; the equipment is: drop hammer impact testing machine. Reference standard GA420-2021 "Police Anti-Riot Clothing" is used to test the impact energy absorption performance (energy absorption mode and absorption rate test); the equipment is: drop hammer impact testing machine.
[0069] Example 1 Preparation of IHP material:
[0070] (1) 100 g of dihydroxy-terminated polydimethylsiloxane (weight average molecular weight of 2000, kinematic viscosity at 25° C. 52 cps) was mixed with 2.5 g of trimethoxyboroxane, and the mixture was stirred at 60° C. for 3 h to obtain a cross-linked product as shown in FIG. (V);
[0071] (2) adding 4 g of diisocyanate to the obtained cross-linked product, reacting at 60° C. for 2 h to obtain an IHP material precursor having a network structure;
[0072] (3) 0.5 g of tetraisopropyl titanate was added to the above-mentioned IHP material precursor, and the IHP material precursor was modified by reacting at 60° C. for 2 h. The product was then subjected to heat treatment (such as hot compression, hot stretching, hot quenching, hot annealing and hot aging, etc.) and mechanical treatment (such as rolling, molding, etc.) to obtain the IHP material.
[0073] Heat treatment and mechanical treatment are currently widely used, and other structures and principles are the same as those in the prior art and will not be described in detail here.
[0074] The IHP material prepared in this example was characterized and tested as follows:
[0075] (1) Morphological characterization:
[0076] SEM characterization was performed on a scanning electron microscope. The sample preparation method used was as follows: the IHP sample was fixed on a silicon wafer, gold-sprayed, and then characterized on a Philips XL 30 ESEM electron microscope (Netherlands).
[0077] The SEM of the IHP material prepared in Example 1 is as follows: Figure 2 shown.
[0078] (2) Performance test:
[0079] Rheology is used to characterize the stress sensitivity of IHP materials; impact energy tester is used to characterize the impact protection performance and energy absorption efficiency of IHP materials.
[0080] Definition of external force sensitivity: The ability of a material to change from soft to hard under mechanical impact is the impact hardening value σ.
[0081] σ=G'max / G'min;
[0082] Where G'max is the maximum value of the storage modulus in the rheological test results, and G'min is the minimum value of the storage modulus in the rheological test results;
[0083] Energy absorption efficiency: During the test, a hammer weighing 5 kg is released at a specified height h and vertically hits the sample placed on the bottom impact force sensor by free fall. The impact velocity at the moment of contact with the sample is determined by the falling height h:
[0084] v 2 =2gh;
[0085] For the blank control group, the force value recorded by the sensor after the impact is recorded as F0 (in N). For the sample, the force value recorded by the sensor after the impact is recorded as F1 (in N). The energy absorption efficiency η expressed by the impact force during the impact process can be calculated using the following formula:
[0086]
[0087] Example 2
[0088] The difference between Example 2 and Example 1 is that the molecular weight of the dihydroxy-terminated polydimethylsiloxane is different, that is, the molecular weight is 5000, and the kinematic viscosity at 25° C. is 82 cps, and the rest of the processes are exactly the same.
[0089] Example 3
[0090] The difference between Example 3 and Example 1 is that the 25° C. kinematic viscosity of the dihydroxy-terminated polydimethylsiloxane is different, that is, the 25° C. kinematic viscosity is 200 cps, and the other processes are exactly the same.
[0091] Example 4
[0092] The difference between Example 4 and Example 1 is that the mass ratio of dihydroxy-terminated polydimethylsiloxane to trimethoxyboroxane is 100:3, and the rest of the processes are exactly the same.
[0093] Example 5
[0094] The difference between Example 5 and Example 1 is that the mass ratio of the dihydroxy-terminated polydimethylsiloxane to trimethoxyboroxane is 100:10, and the other processes are exactly the same.
[0095] Example 6
[0096] The difference between Example 5 and Example 1 is that the mass ratio of the dihydroxy-terminated polydimethylsiloxane to trimethoxyboroxane is 100:1, and the other processes are exactly the same.
[0097] Example 7
[0098] The difference between Example 5 and Example 1 is that the mass ratio of dihydroxy-terminated polydimethylsiloxane to trimethoxyboroxane is 80:1, and the rest of the processes are exactly the same.
[0099] Example 8
[0100] The difference between Example 8 and Example 1 is that the mass ratio of the dihydroxy-terminated polydimethylsiloxane to diisocyanate is 100:1, and the rest of the processes are exactly the same.
[0101] Example 9
[0102] The difference between Example 9 and Example 1 is that the mass ratio of the dihydroxy-terminated polydimethylsiloxane to diisocyanate is 20:1, and the rest of the processes are exactly the same.
[0103] Example 10
[0104] The difference between Example 10 and Example 1 is that the reaction temperature in step (1) is different, the reaction temperature is 80° C., and the rest of the processes are exactly the same.
[0105] Comparative Example 1
[0106] The difference between Comparative Example 1 and Example 1 is that the reaction raw materials are different, and diamino-terminated polydimethylsiloxane is used instead of dihydroxy-terminated polydimethylsiloxane, and the rest of the processes are exactly the same.
[0107] Comparative Example 2
[0108] The difference between Comparative Example 2 and Example 1 is that the boron-containing cross-linking agent is different, and boric acid is used instead of trimethoxyboroxane, and the rest of the processes are exactly the same.
[0109] The characterization methods and results of the IHP materials prepared in Examples 2 to 10 are equivalent to those in Example 1 and will not be described in detail here.
[0110] The performance of the IHP materials prepared in Examples 1 to 10 and the materials prepared in Comparative Examples 1 to 2 were tested, and the structural parameters of the IHP materials were characterized by SEM; the external stress resistance and self-healing ability of the IHP materials were characterized by rheology and DMTA; the impact protection performance, energy absorption efficiency and mode of the IHP materials were characterized by an impact energy tester, and the test results are shown in Table 1.
[0111] Table 1 Impact protection performance, energy absorption efficiency and mode detection results of IHP materials
[0112]
[0113] As can be seen from Table 1, the molecular weight and 25°C kinematic viscosity of the dihydroxy-terminated polydimethylsiloxane have the greatest influence on the performance of the product. As the molecular weight of the polydimethylsiloxane decreases, the external force sensitivity and energy absorption efficiency of the prepared IHP material are improved at the same time. In particular, the prepared material has good energy absorption efficiency and intelligent response characteristics to external forces. When the molecular weight of the dihydroxy-terminated polydimethylsiloxane obtained in Example 1 is 2000 and the 25°C kinematic viscosity is 52 cst, the prepared IHP material has the best performance.
[0114] As shown in the data in Table 1, changing the ratio of dihydroxy-terminated polydimethylsiloxane to trimethoxyboroxane also has a great influence on the performance of the product. As the ratio of the two increases, the impact resistance of the material is improved to a certain extent. When the ratio is 100:2.5, the maximum improvement effect is achieved, about 93.5.
[0115] Example 11 Construction of a bicontinuous IPN composite material:
[0116] 50 g of the sample of Example 1 was taken as the first continuous phase, and 30 g of polysiloxane (molecular weight 20,000) was taken as the second continuous phase, and the mixture was mixed and reacted at 60° C. for 2 to 3 h to construct a dual-continuous IPN composite system.
[0117] The following characterization and testing were performed on the bicontinuous IPN composite system prepared in this example:
[0118] The test of the dual continuous IPN composite system is the same as that of the IHP material in Example 1.
[0119] Example 12
[0120] Example 12 is different from Example 11 in that the second continuous phase is hydroxy MQ resin with a molecular weight of 20,000, and the rest of the processes are exactly the same.
[0121] Embodiment 13
[0122] The difference between Example 13 and Example 11 is that the mass ratio of the first continuous phase to the second continuous phase is different, that is, the mass ratio of the first continuous phase to the second continuous phase is 1:1, and the rest of the processes are exactly the same.
[0123] Embodiment 14
[0124] The difference between Example 14 and Example 11 is that the mass ratio of the first continuous phase to the second continuous phase is different, that is, the mass ratio of the first continuous phase to the second continuous phase is 1:0.5, and the rest of the processes are exactly the same.
[0125] Embodiment 15
[0126] The difference between Example 15 and Example 11 is that the reaction conditions are different, the reaction temperature is 80° C., and the rest of the processes are exactly the same.
[0127] Comparative Example 3
[0128] The difference between Comparative Example 3 and Example 11 is that the first continuous phase is different, and the sample of Example 2 is used as the first continuous phase, and the rest of the processes are exactly the same.
[0129] The demonstration methods and results of the dual continuous IPN composite systems prepared in Examples 12 to 14 are equivalent to those in Example 11 and will not be repeated here.
[0130] The performance of the IHP materials and the bicontinuous IPN composite system prepared in Examples 11 to 14 and the materials prepared in Comparative Examples 3 to 5 were tested. The structural parameters of the bicontinuous IPN composite system were characterized by SEM. The external stress capacity and self-healing ability of the IHP material were characterized by rheology and DMTA. The impact protection performance, energy absorption efficiency and mode of the IHP material were characterized by an impact energy tester. The test results are shown in Table 2.
[0131] Table 2 Impact protection performance, energy absorption efficiency and mode detection results of IHP materials
[0132]
[0133] It can be seen from Table 2 that the molecular weight of the IHP material and the mass ratio of the first continuous phase to the second continuous phase have the greatest influence on the performance of the product. With the increase of the molecular weight of the IHP material, the external force sensitivity and energy absorption efficiency of the prepared bicontinuous IPN composite system are improved at the same time. In particular, the prepared material has good energy absorption efficiency and intelligent response characteristics to external force. Among them, the bicontinuous IPN composite system prepared by the IHP material in Example 11 has the best performance. Moreover, the dual-continuous IPN composite system prepared in the present application has excellent intelligent protection performance, and the impact test transmission force value is ≤35kN (impact energy is 50J); the dual-continuous IPN composite system is kept for 4 hours in a low temperature environment of -23℃±2℃ and a high temperature environment of ﹢50℃±5℃, and the impact force value is 3J, and the sensing impact force should be ≤6KN. The test method adopts the GB / T 2812-2006B standard; it is kept for 4 hours in a normal temperature environment of 23℃±2℃ and a low temperature environment of -50°±2°, and then taken out and folded up and down 10,000 times, and there is no delamination, deformation or bulging, breakage or damage in appearance.
[0134] Example 16 Preparation of three-dimensional impact protection material:
[0135] Weigh 10 g of the bicontinuous IPN composite material prepared in Example 11, 100 g of EVA resin, 10 g of polyurethane black and white material, 1 g of vulcanizing agent, 6 g of coupling agent, and 0.8 g of foaming agent, and mix them at 90° C. to prepare an EVA / IHP blend material;
[0136] The above blended material was molded and foamed for 8 minutes under 18 MPa to prepare a three-dimensional impact protection foam material for sports protection.
[0137] Sample impact protection performance test: The impact protection performance test of protective materials is carried out in accordance with the EU standard BS EN1621-1:2012. The lower the force value transmitted, the better the material protection performance. Test equipment: Drop weight impact tester
[0138] Calculation method of impact energy absorption efficiency: Energy absorption efficiency of materials at different impact heights % = (theoretical impact energy at this height - impact energy transmitted to the lower sensor) / theoretical impact energy at this height; Test equipment: drop hammer impact tester
[0139] Embodiment 17
[0140] The difference between Example 17 and Example 16 is that the mass ratio of the bicontinuous IPN composite material to the EVA foaming material is different, that is, the mass ratio is 20:100, and the rest of the processes are exactly the same.
[0141] Embodiment 18
[0142] The difference between Example 18 and Example 16 is that the mass ratio of the bicontinuous IPN composite material (Example 16) to the EVA foam material is different, that is, the mass ratio is 25:100, and the rest of the processes are exactly the same.
[0143] Embodiment 19
[0144] The difference between Example 19 and Example 16 is that the formula of the foaming material is different. The foaming material includes 10g of bicontinuous IPN composite material, 100g of EVA resin, 25g of polyurethane black and white material, 1.5g of vulcanizing agent, 8g of coupling agent, and 0.6g of foaming agent. The rest of the processes are exactly the same.
[0145] Embodiment 20
[0146] The difference between Example 20 and Example 16 is that the IHP material is used to replace the bicontinuous IPN composite material, and the other processes are exactly the same.
[0147] Comparative Example 4
[0148] The difference between Comparative Example 4 and Example 16 is that the IHP material and the bicontinuous IPN composite material are not added, and the other processes are exactly the same.
[0149] The three-dimensional impact protection materials prepared in Examples 16 to 20 and the material of Comparative Example 4 were tested for performance, and the test results are shown in Table 3 below:
[0150] Table 3
[0151]
[0152]
[0153] It can be seen from Table 3 that the ratio of IHP material or bicontinuous IPN composite material to EVA foam material has the greatest impact on the performance of the product. As the proportion of IHP material or bicontinuous IPN composite material increases, the external force sensitivity and impact protection performance of the prepared three-dimensional impact protection material are also improved. Among them, the three-dimensional impact protection material prepared by Example 18 has the best performance and reaches the EU safety protection level 1 standard. The three-dimensional impact protection material prepared in this application can be used as a sports protection material, and the application includes as a lining for helmets and / or sports protection items such as knee pads, elbow pads, yoga mats, sports fabrics, etc., and can also be made into textiles for sports protection. The tearing force of the product is ≥15N; Flame retardant performance: Use a Bunsen burner perpendicular to the blue flame for a flame retardant test and leave the flame after ten seconds. It can be extinguished after 5 seconds, and the flame retardant grade reaches FV-0.
[0154] In summary, the present application uses hydroxyl-terminated polydimethylsiloxane and trimethoxyboryl hexacyclic ring as the main raw materials, diisocyanate as the chemical linking point, and tetraisopropyl titanate as the hydrolysis modifier to prepare IHP materials and bicontinuous IPN composite materials, construct three-dimensional composite protective materials, and apply the three-dimensional composite protective materials to fabrics for sports protection. The results show that in addition to the aforementioned excellent external force sensitivity and negative Poisson's ratio, the synthesized IHP materials and bicontinuous IPN composite materials also have excellent self-healing ability. In 20 cycle tests, the attenuation of the mechanical properties of the material was less than 30%, and the external force sensitivity showed a certain increasing trend, up to 6000-10000 times. This shows that IHP materials and bicontinuous IPN composite materials have good self-healing properties. At the same time, the impact test results of the three-dimensional composite protective material constructed using IHP materials and bicontinuous IPN composite materials show that the impact performance of the three-dimensional composite protective material increases significantly with the increase of the external force impact speed, and the energy absorption efficiency can reach about 78%, which is significantly better than the performance of the existing sports protection products.
[0155] The above examples are for the purpose of illustrating the embodiments disclosed in the present application and should not be construed as limiting the present application. In addition, the various modifications listed herein and the changes in the methods and compositions in the application are obvious to those skilled in the art without departing from the scope and spirit of the present application. Although the present application has been specifically described in conjunction with a variety of specific preferred embodiments of the present application, it should be understood that the present application should not be limited to these specific embodiments. In fact, various modifications as described above that are obvious to those skilled in the art to obtain the application should be included in the scope of the present application.
Claims
1. A three-dimensional impact-resistant protective material, characterized in that: It is prepared from raw materials comprising the following components in parts by weight: The bicontinuous IPN composite material is a network polymer constructed by mixing and reacting at 60° C. for 2 to 3 hours with a silicon-boron-containing IHP material as the first continuous phase and one or more of polysiloxane, branched MQ resin or thermoplastic elastomer as the second continuous phase.
2. A three-dimensional impact-resistant protective material according to claim 1, characterized in that: It is prepared from raw materials comprising the following components in parts by weight: The bicontinuous IPN composite material is a network polymer constructed by mixing and reacting at 60° C. for 2 to 3 hours with a silicon-boron-containing IHP material as the first continuous phase and one or more of polysiloxane, branched MQ resin or thermoplastic elastomer as the second continuous phase.
3. The three-dimensional impact-resistant protective material according to claim 1, characterized in that: The structure of the IHP material is shown in formula (I):
4. The three-dimensional impact-resistant protective material according to claim 1, characterized in that: The vulcanizing agent is BIBP; the coupling agent is KH-570; and the foaming agent is AC3000h.
5. A method for preparing a three-dimensional impact-resistant protective material according to any one of claims 1 to 4, characterized in that: The following steps are involved: Step 1: Preparation of IHP materials: (1) reacting polysiloxane with a boron-containing crosslinking agent at 50 to 90° C. for 3 to 6 hours to obtain a crosslinked product; the mass ratio of the polysiloxane to the boron-containing crosslinking agent is 10 to 100:1; (2) mixing the cross-linked product with a chain extender, reacting at 60 to 9° C. for 2 to 6 hours, to obtain an IHP material precursor having a network structure; the ratio of the polysiloxane to the chain extender is 20 to 100:1; (3) heat treating, solvating and / or mechanically treating the IHP material precursor to prepare the IHP material; Step 2, preparing a bicontinuous IPN composite material: using an IHP material as a first continuous phase, and using one or more of polysiloxane, branched MQ resin or thermoplastic elastomer as a second continuous phase, mixing and reacting at 60° C. for 2 to 3 hours to prepare a bicontinuous IPN composite material; wherein the mass ratio of the first continuous phase to the second continuous phase is 1:0.2 to 5; Step 3, preparing a three-dimensional impact protection material: using IHP material and / or bicontinuous IPN composite material as a dispersed body and EVA foam material as a carrier, performing banburying and blending to prepare EVA / IHP blended material, and then forming the EVA / IHP blended material into a three-dimensional impact protection material by foaming molding; wherein the mass ratio of the dispersed body to the EVA foam material is 5-30:60-110.
6. The preparation method according to claim 5, characterized in that: In step 1(1), the polysiloxane is one or more of bishydroxy-terminated polydimethylsiloxane, bisamino-terminated polydimethylsiloxane, vinyl-terminated hydroxyl-terminated polydimethylsiloxane, vinyl-terminated amino-polydimethylsiloxane, hydrogen-terminated hydroxyl-terminated polydimethylsiloxane, hydrogen-terminated amino-polydimethylsiloxane and vinyl-terminated hydrogen-terminated polydimethylsiloxane.
7. The preparation method according to claim 6, characterized in that: The polysiloxane is dihydroxy-terminated polydimethylsiloxane with a weight average molecular weight of 1000-20000 and a viscosity of 20-200 cps.
8. The preparation method according to claim 7, characterized in that: The boron-containing cross-linking agent is one or more of borates, boric acid compounds, boric acid esters and trimethoxyboroxane.
9. The preparation method according to claim 5, characterized in that: In step 3, the EVA foam material comprises the following parts by weight: 5-30 parts of bicontinuous IPN composite material, 60-110 parts of EVA resin, 5-30 parts of polyurethane black and white material, 0.5-5 parts of vulcanizing agent, 0.5-7 parts of coupling agent, and 0.5-2 parts of foaming agent.
10. Use of the three-dimensional impact-resistant protective material according to any one of claims 1 to 4 or the three-dimensional impact-resistant protective material prepared by the preparation method of the three-dimensional impact-resistant protective material according to claim 5 in sports protective materials.
Citation Information
Patent Citations
Preparation method of intelligent stress response material
CN103113591A
Supramolecular polyurethane impact-resistant material containing multiple hydrogen bonds and preparation method of supramolecular polyurethane impact-resistant material
CN111848907A
Impact-resistant protective material and preparation method thereof
CN113429797A
Preparation method of self-healing impact-resistant organic hydrogel with speed responsiveness
CN118126259A
Method for preparing intelligent stress response type silicon-boron polymer micro-gel