Additional asphalt mixture modifier as well as preparation method and application thereof

Through the dry process of using components such as polyolefins, rubber materials and inorganic adhesives in asphalt mixtures, the problems of existing modifiers in weather resistance, low temperature performance and water damage resistance are solved, and the high modifiers are achieved Performance and low energy consumption process, suitable for paving technology of asphalt pavement.

CN118909344APending Publication Date: 2024-11-08GUANGSHENZHU EXPRESSWAY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410974860.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Existing asphalt mixture modifiers perform poorly in weather resistance, low temperature performance and water damage resistance, and have problems of high energy consumption and environmental pollution.

Method used

The external asphalt mixture modifier is prepared by dry process using polyolefins, rubber materials, anti-flaking agents, cold-resistant agents, weather-resistant agents and lubricants. The low melting point of polyolefins and the thermoplasticity of rubber materials are used. Combining inorganic adhesives and cold-resistant agents improves the dispersion and low-temperature resistance of the modifier.

Benefits of technology

The modifier has achieved good water damage resistance, low temperature and rut resistance, simplified the process flow, reduced energy consumption, and improved the comprehensive performance of the asphalt mixture.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004954244390000101
    Figure BDA0004954244390000101
  • Figure BDA0004954244390000111
    Figure BDA0004954244390000111
  • Figure BDA0004954244390000121
    Figure BDA0004954244390000121
Patent Text Reader

Abstract

The invention discloses an externally-doped asphalt mixture modifier as well as a preparation method and application thereof. The externally-doped asphalt mixture modifier comprises 75%-95% of polyolefin, 0-15% of a rubber material, 0-1.0% of an anti-stripping agent, 0-5% of a cold-resistant agent, 0.3%-0.5% of a weather-resistant agent, 0.4%-0.8% of a heat-resistant agent and 0.5%-1.5% of a lubricant. The asphalt pavement material has the advantages of good comprehensive performance such as water damage resistance, rut resistance and low-temperature performance, and can be popularized and applied to the paving technology of asphalt pavements. Compared with the traditional wet process, the dry process disclosed by the invention is simpler in process, lower in energy consumption, convenient to use and very wide in application prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of asphalt modification, and in particular to an externally-admixed asphalt mixture modifier and a preparation method and application thereof. Background Art

[0002] HMA (Hot Mixture Asphalt) refers to an asphalt pavement construction process in which asphalt mixture is mixed, spread and rolled at a relatively high temperature. Hot mix asphalt pavement accounts for more than 94% in the United States. Hot mix asphalt mixture is widely used in highway construction in my country. In its construction process, the asphalt is heated at about 160℃~165℃, and the mineral material is generally heated at 180℃~190℃. The mixture is hot mixed and the temperature is about 170℃~180℃. Heating asphalt and mineral materials to such a high temperature not only consumes a lot of energy, but also produces a lot of CO2, smoke and harmful gases in the production process, which seriously affects the surrounding environment and the health of construction workers.

[0003] In the prior art, Chinese invention patent application CN201310013993.1 discloses an environmentally friendly asphalt mixture modifier, which selects polyethylene wax as the main base material. However, due to the low molecular weight, it has poor heat resistance and weathering aging performance; while Chinese invention patent application CN201110212562.9 discloses an asphalt mixture warm mix modifier prepared by using waste plastics and inorganic reinforcing agents. The base material is all waste plastics, which has the problems of unstable performance and poor aging resistance. At the same time, the inorganic reinforcing agent has the defects of poor reinforcement effect and poor compatibility.

[0004] Therefore, in view of the shortcomings of existing modifiers, there is an urgent need for an externally-admixed asphalt mixture modifier with better comprehensive properties such as weather resistance, low temperature performance, and water damage resistance. Summary of the invention

[0005] The purpose of the present invention is to provide an externally-admixed asphalt mixture modifier and a preparation method and application thereof, which has excellent water damage resistance, excellent low temperature performance and good rutting resistance, and better solves the problems existing in the prior art.

[0006] In order to achieve the above object, the present invention adopts the following technical solutions:

[0007] In the first aspect, the present invention provides an externally-admixed asphalt mixture modifier, which comprises the following components by weight percentage: 75% to 95% polyolefin, 0% to 15% rubber material, 0% to 1.0% anti-stripping agent, 0% to 5% cold-resistant agent, 0.3% to 0.5% weather-resistant agent, 0.4% to 0.8% heat-resistant agent and 0.5% to 1.5% lubricant.

[0008] As one of the preferred technical solutions of the present invention, the external asphalt mixture modifier includes the following components by weight percentage: 77% to 84.5% of polyolefin, 7.5% to 15% of rubber material, 0.5% to 1.0% of anti-stripping agent, 2.5% to 5% of cold-resistant agent, 0.3% to 0.5% of weather-resistant agent, 0.4% to 0.8% of heat-resistant agent and 0.5% to 1.5% of lubricant.

[0009] As one of the specific technical solutions of the present invention, the polyolefin is one or two of low-density polyethylene, linear low-density polyethylene, and high-density polyethylene. The technical index requirements of polyolefin are: granular, with a particle size of 1 to 3 mm; a melting point of 100°C to 115°C; and a melt index of 1 to 20 g / 10 min.

[0010] Preferably, the polyolefin is obtained by blending low-density polyethylene and linear low-density polyethylene in a blending ratio of (1:3) to (3:1).

[0011] Preferably, the blending ratio of low density polyethylene to linear low density polyethylene is 1:2.

[0012] As one of the specific technical solutions of the present invention, the rubber material is thermoplastic elastomer rubber. Specific requirements of the rubber material: hardness of 20-60D; filling amount ≤20%.

[0013] Preferably, the rubber material is an unvulcanized rubber material, and the rubber material is selected to be applicable to the fields of headphone wires, rubber bands, children's rubber toys, etc.

[0014] As one of the specific technical solutions of the present invention, the anti-stripping agent is an inorganic adhesive. Specific parameters of the anti-stripping agent: specific surface area ≥ 300m 2 / kg; particle size (80 micron square hole) ≤10%; strength ≥42.5R.

[0015] Preferably, the anti-stripping agent is a silicate adhesive.

[0016] As one of the specific technical solutions of the present invention, the cold-resistant agent is automobile lubricating oil or furfural oil. The technical index requirements of the cold-resistant agent are: kinematic viscosity (100°C) is between 20 and 120 mm 2 / s; aromatic hydrocarbon content is >80%.

[0017] Preferably, the cold-resistant agent is furfural oil, which has a cold-resistant effect and significantly improves the low-temperature resistance of asphalt mixture.

[0018] As one of the specific technical solutions of the present invention, the weathering agent is at least one of an ultraviolet absorber and a light stabilizer.

[0019] Preferably, the weathering agent is a mixture of an ultraviolet absorber and a light stabilizer, and the compounding ratio is 1:1; the ultraviolet absorber is a benzotriazole ultraviolet absorber; and the light stabilizer is a hindered amine light stabilizer.

[0020] As one of the specific technical solutions of the present invention, the heat-resistant agent is a blend of tris(2,4-di-tert-butylbenzene)phosphite and pentaerythritol tetrakis[β-(3.5-di-tert-butyl-4-hydroxyphenyl)propionate] in a mixing mass ratio of 1:2, which can better prevent the modifier from thermal aging during preparation and use.

[0021] As one of the specific technical solutions of the present invention, the lubricant is any one of ethylene bis stearamide lubricants, polyolefin wax, and stearic acid lubricants. The lubricant has a lubricating effect, which helps to disperse and mix the modifier during processing, improve production efficiency and reduce energy consumption; and, during use, it helps to disperse the modifier.

[0022] In a second aspect, the present invention provides a method for preparing the above-mentioned externally-admixed asphalt mixture modifier, comprising the following steps:

[0023] Step 1: Heat the cold-resistant agent to 80℃~100℃;

[0024] Step 2: Put polyolefin, rubber material, anti-stripping agent, weathering agent, heat-resistant agent and lubricant into a mixing tank in order by weight, then add the cold-resistant agent in step 1, and stir at a stirring speed of 400 to 600 r / min for 2 to 4 minutes to obtain a uniform mixture;

[0025] Step 3: Add the mixture obtained in step 2 to a twin-screw extruder for plasticization, shearing, and melting to form a uniform melt. The extrusion temperature is set to 120-150°C, the vacuum degree is -0.1-0.04MPa, and the screw speed is set to 350-500r / min. The melt is pulled through the extrusion die, and then cooled, dried, blown dry, and pelletized to obtain modifier particles.

[0026] In a third aspect, the present invention also provides the use of the above-mentioned externally-admixed asphalt mixture modifier in a dry externally-admixed asphalt mixture.

[0027] Compared with the prior art, the present invention provides an externally-admixed asphalt mixture modifier and a preparation method and application thereof, which have the following beneficial effects:

[0028] The present invention adopts polyolefins with the advantages of low melting point and easy dispersion, adopts unvulcanized thermoplastic elastomers with good performance, and compounded cold-resistant agents to improve the low-temperature resistance of the product; in addition, the present invention innovatively uses inorganic silicate adhesives to improve the water damage resistance of the product. The product using the present invention has the advantages of good comprehensive performance such as water damage resistance, rutting resistance, and low-temperature performance, and can be promoted and applied to asphalt pavement paving technology.

[0029] The product of the present invention optimizes the traditional process from the "two-step method" to the "one-step method" and from the "wet method" to the "dry method". The present invention provides an "external admixture" modifier. In the production process of asphalt mixture, the modifier is directly added to the asphalt mixture mixing pot for mixing, and the shear force generated during the mixing process is used for dispersion. After mixing with stone (dry mixing), asphalt is added and mixed together (wet mixing), so that the modifier is fully dispersed in the asphalt mixture to play a modification role.

[0030] The present invention directly mixes the modifier, asphalt and aggregate, referred to as the "dry process", also known as the "one-step process", to obtain a modified asphalt mixture with excellent performance. The traditional process has two major steps, called the "wet process", also known as the "two-step process": 1. Prepare the modified asphalt first; 2. Mix the modified asphalt with the aggregate; The first step of the traditional process, the preparation of modified asphalt, is a complex process that requires a lot of energy consumption, including the storage of modified asphalt, the stability and control of asphalt performance, etc. Compared with the "wet process", the "dry process" of the present invention is simpler, reduces energy consumption, is easy to use, and has a very broad application prospect. DETAILED DESCRIPTION

[0031] The technical solution of the present invention will be described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0032] The present invention provides an externally mixed asphalt mixture modifier, which comprises the following components by weight percentage: 77% to 84.5% of polyolefin, 7.5% to 15% of rubber material, 0.5% to 1.0% of anti-stripping agent, 2.5% to 5% of cold-resistant agent, 0.3% to 0.5% of weather-resistant agent, 0.4% to 0.8% of heat-resistant agent and 0.5% to 1.5% of lubricant.

[0033] In some embodiments, the polyolefin can be selected from one or two of low-density polyethylene, linear low-density polyethylene, and high-density polyethylene. The technical indicators of the polyolefin are as follows: granular, with a particle size of 1 to 3 mm; a melting point of 100°C to 115°C; and a melt index of 1 to 20 g / 10 min. As an example, the polyolefin is obtained by blending low-density polyethylene and linear low-density polyethylene, and the blending ratio is (1:3) to (3:1).

[0034] In some embodiments, the rubber material may be thermoplastic elastomer rubber. Specific requirements for the rubber material: hardness of 20 to 60D; filling amount ≤ 20%. As an example, the rubber material is an unvulcanized rubber material that can be used in the fields of headphone wires, rubber straps, children's rubber toys, etc.

[0035] In some embodiments, the anti-stripping agent may be an inorganic adhesive. Specific parameters of the anti-stripping agent: specific surface area ≥ 300m 2 / kg; particle size (80 micrometer square hole) ≤ 10%; strength ≥ 42.5R. As an example, the anti-stripping agent adopts a silicate adhesive.

[0036] In some embodiments, the cold-resistant agent can be selected from automotive lubricating oil or furfural oil. The technical index requirements of the cold-resistant agent are: kinematic viscosity (100°C) is between 20 and 120 mm 2 / s; aromatic hydrocarbon content is> 80%. As an example, the cold-resistant agent is furfural oil.

[0037] In some embodiments, the weathering agent may be at least one of an ultraviolet absorber and a light stabilizer. As an example, the weathering agent is a mixture of an ultraviolet absorber and a light stabilizer, and the compounding ratio is 1:1; the ultraviolet absorber is a benzotriazole ultraviolet absorber; and the light stabilizer is a hindered amine light stabilizer.

[0038] In some embodiments, the heat-resistant agent can be a blend of tris(2,4-di-tert-butylbenzene)phosphite and pentaerythritol tetrakis[β-(3.5-di-tert-butyl-4-hydroxyphenyl)propionate] in a mass ratio of 1:2. The lubricant can be any one of ethylene bisstearamide lubricants, polyolefin wax, and stearic acid lubricants.

[0039] The preparation method of the externally mixed asphalt mixture modifier comprises the following steps:

[0040] Step 1: Heat the cold-resistant agent to 80℃~100℃;

[0041] Step 2: Put polyolefin, rubber material, anti-stripping agent, weathering agent, heat-resistant agent and lubricant into a mixing tank in order by weight, then add the cold-resistant agent in step 1, and stir at a stirring speed of 400 to 600 r / min for 2 to 4 minutes to obtain a uniform mixture;

[0042] Step 3: Add the mixture obtained in step 2 to a twin-screw extruder for plasticization, shearing, and melting to form a uniform melt. The extrusion temperature is set to 120-150°C, the vacuum degree is -0.1-0.04MPa, and the screw speed is set to 350-500r / min. The melt is pulled through the extrusion die, and then cooled, dried, blown dry, and pelletized to obtain modifier particles.

[0043] The present invention is further described in detail below through detailed examples.

[0044] In the embodiments and comparative examples, the experimental methods used are conventional methods unless otherwise specified, and the materials, reagents, etc. used are all commercially available unless otherwise specified.

[0045] Example 1

[0046] The present embodiment provides an externally-admixed asphalt mixture modifier, which comprises the following components by weight percentage: 77.5% polyolefin, 15% rubber material, 0.5% anti-stripping agent, 5% cold-resistant agent, 0.4% weather-resistant agent, 0.6% heat-resistant agent and 1% lubricant.

[0047] Among them, polyolefin is obtained by blending low-density polyethylene and linear low-density polyethylene, and the blending ratio is 1: 2. The technical index requirements of polyolefin are: granular, particle size is 1 to 3 mm; melting point is 100℃ to 115℃; melt index is 1 to 20g / 10min.

[0048] The rubber material adopts unvulcanized thermoplastic elastomer rubber, and its specific requirements are: hardness of 20-60D; filling amount ≤20%; specifically, the rubber material selection can be applied to rubber materials in the fields of headphone wires, rubber straps, children's rubber toys, etc.

[0049] The anti-stripping agent adopts silicate adhesive; the specific parameters of the anti-stripping agent: specific surface area ≥ 300m 2 / kg; particle size (80 micron square hole) ≤10%; strength ≥42.5R.

[0050] The cold-resistant agent uses furfural oil, and its technical index requirements are: kinematic viscosity (100℃) is between 20 and 120 mm 2 / s; aromatic hydrocarbon content is >80%.

[0051] The weathering agent is a mixture of an ultraviolet absorber and a light stabilizer, and the compounding ratio is 1:1; the ultraviolet absorber adopts a benzotriazole ultraviolet absorber; the light stabilizer adopts a hindered amine light stabilizer.

[0052] The heat-resistant agent is a blend of tris(2,4-di-tert-butylbenzene)phosphite and pentaerythritol tetrakis[β-(3.5-di-tert-butyl-4-hydroxyphenyl)propionate] in a mixing mass ratio of 1:2.

[0053] The lubricant is ethylene bis stearamide lubricant.

[0054] Specifically, the preparation method of the external asphalt mixture modifier comprises the following steps:

[0055] Step 1: Heat the cold-resistant agent to 90°C;

[0056] Step 2: Put polyolefin, rubber material, anti-stripping agent, weathering agent, heat-resistant agent and lubricant into a mixing tank in order by weight, then add the cold-resistant agent in step 1, and stir at a stirring speed of 500 r / min for 3 minutes to obtain a uniform mixture;

[0057] Step 3: Add the mixture obtained in step 2 to a twin-screw extruder for plasticization, shearing, and melting to form a uniform melt. The extrusion temperature is set to 140°C, the vacuum degree is -0.08MPa, and the screw speed is set to 400r / min. The melt is pulled through the extrusion die and then cooled, dried, blown dry, and pelletized to obtain modifier particles.

[0058] Example 2

[0059] This embodiment provides an externally mixed asphalt mixture modifier, which includes the following components by weight percentage: 77% polyolefin, 15% rubber material, 1% anti-stripping agent, 5% cold-resistant agent, 0.4% weather-resistant agent, 0.6% heat-resistant agent and 1% lubricant. The selection of specific components and the preparation method are the same as those in Example 1.

[0060] Example 3

[0061] This embodiment provides an external asphalt mixture modifier, which includes the following components by weight percentage: 84.5% polyolefin, 7.5% rubber material, 1% anti-stripping agent, 5% cold-resistant agent, 0.4% weather-resistant agent, 0.6% heat-resistant agent and 1% lubricant. The selection of specific components and the preparation method are the same as those in Example 1.

[0062] Example 4

[0063] This embodiment provides an external asphalt mixture modifier, which includes the following components by weight percentage: 79.5% polyolefin, 15% rubber material, 1% anti-stripping agent, 2.5% cold-resistant agent, 0.4% weather-resistant agent, 0.6% heat-resistant agent and 1% lubricant. The selection of specific components and the preparation method are the same as those in Example 1.

[0064] Comparative Example 1

[0065] This comparative example provides an externally mixed asphalt mixture modifier, which includes the following components by weight percentage: 92.5% polyolefin, 0.5% anti-stripping agent, 5% cold-resistant agent, 0.4% weather-resistant agent, 0.6% heat-resistant agent and 1% lubricant. The selection of specific components is the same as that of Example 1, and the preparation method is the same as that of Reference Example 1.

[0066] Comparative Example 2

[0067] This comparative example provides an externally mixed asphalt mixture modifier, which includes the following components by weight percentage: 78% polyolefin, 15% rubber material, 5% cold-resistant agent, 0.4% weather-resistant agent, 0.6% heat-resistant agent and 1% lubricant. The selection of specific components is the same as that of Example 1, and the preparation method is the same as that of Reference Example 1.

[0068] Comparative Example 3

[0069] This comparative example provides an externally mixed asphalt mixture modifier, which includes the following components by weight percentage: 82.5% polyolefin, 15% rubber material, 0.5% anti-stripping agent, 0.4% weathering agent, 0.6% heat-resistant agent and 1% lubricant. The selection of specific components is the same as that of Example 1, and the preparation method is the same as that of Reference Example 1.

[0070] 1. The melt index and softening point of the modifiers prepared in Examples 1 to 4 and Comparative Examples 1 to 3 were tested, and the test data are shown in Table 1. The softening point was obtained by mixing 6% of the modifier into 70# base asphalt according to the "Testing Procedures for Asphalt and Asphalt Mixtures for Highway Engineering" T0606-2011.

[0071] Table 1 Melt index and softening point test results

[0072]

[0073] 2. The modifiers prepared in Examples 1 to 4 and Comparative Examples 1 to 3 were applied to the preparation of dry-mixed asphalt mixtures, and corresponding test samples were prepared to test their performance.

[0074] The indoor test method ("dry" process) is adopted, and the specific process is as follows:

[0075] (1) A total of nine tests, Test 1 to Test 9, were set up for testing. Among them, Test 1 to Test 3 were respectively tested using the modifiers obtained in Comparative Examples 1 to 3 and Esso 70# base asphalt, Test 4 was tested using Esso 70# base asphalt, Test 5 was tested using SBS modified asphalt (a commercial product that meets the ID national standard, with a softening point of more than 80°C), and Test 6 to Test 9 were respectively tested using the modifiers obtained in Examples 1 to 4 and Esso 70# base asphalt. The specific asphalt mixture proportions are shown in Table 2 below.

[0076] (2) The AC-13 graded stone material is heated at 170-190℃ / 4-6H; the 70# base asphalt is heated at 130-140℃ / 1-2H; and the SBS modified asphalt is heated at 170-180℃ / 1-2H.

[0077] (3) Add the corresponding modifier and Esso 70# base asphalt into AC-13 graded stone and stir for 120 to 160 seconds at a mixing temperature of 170 to 180°C.

[0078] (4) Add mineral powder and mix for 80 to 120 seconds at a mixing temperature of 170 to 180°C.

[0079] (5) Prepare test molds such as Marshall, rutting, and beam bending.

[0080] Table 2 Asphalt mixture ratio

[0081]

[0082]

[0083] The data of each test are shown in Table 3 below.

[0084] Table 3 Test data

[0085]

[0086] From the data in Table 1 and Table 3, it can be seen that since rubber materials, anti-stripping agents and cold-resistant agents are added to the formulas of Examples 1 to 4, the corresponding tests 6 to 9 have good comprehensive performance, which is excellent in water damage resistance, low temperature performance and good rutting resistance; the addition of anti-stripping agents improves the water damage resistance and cold resistance, but the addition ratio cannot be increased all the time, which will affect the low temperature resistance, and should be controlled within a certain suitable addition range; rubber materials and cold-resistant agents promote the low temperature performance and processing performance of the materials, but have a certain impact on the high temperature performance and water damage performance. The proportion design of the material formula requires each additive to find the best balance point so that the performance of the mixture reaches the optimal value. The present invention optimizes the dosage ratio of each component, so that the comprehensive performance of the product is better than that of the conventional SBS modified asphalt mixture, so that it is convenient to use, low cost and has the effect of energy saving and consumption reduction when applied in the "dry process".

[0087] The above embodiments are merely illustrative of the concept and technical solution of the present invention, and are not intended to limit the present invention. Anyone familiar with the technology may modify or change the above embodiments without violating the spirit and scope of the present invention. Therefore, all equivalent modifications or changes made by a person with ordinary knowledge in the technical field without departing from the spirit and technical ideas disclosed by the present invention should still be covered by the claims of the present invention.

[0088] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This narrative method of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each implementation mode may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.

Claims

1. An external asphalt mixture modifier, characterized in that: The invention comprises the following components by weight percentage: 75% to 95% of polyolefin, 0% to 15% of rubber material, 0% to 1.0% of anti-stripping agent, 0% to 5% of cold-resistant agent, 0.3% to 0.5% of weather-resistant agent, 0.4% to 0.8% of heat-resistant agent and 0.5% to 1.5% of lubricant.

2. The externally-admixed asphalt mixture modifier according to claim 1, characterized in that: The invention comprises the following components by weight percentage: 77% to 84.5% of polyolefin, 7.5% to 15% of rubber material, 0.5% to 1.0% of anti-stripping agent, 2.5% to 5% of cold-resistant agent, 0.3% to 0.5% of weather-resistant agent, 0.4% to 0.8% of heat-resistant agent and 0.5% to 1.5% of lubricant.

3. The externally-admixed asphalt mixture modifier according to claim 1, characterized in that: The polyolefin is one or two of low-density polyethylene, linear low-density polyethylene, and high-density polyethylene.

4. The externally-admixed asphalt mixture modifier according to claim 3, characterized in that: The polyolefin is obtained by blending low-density polyethylene and linear low-density polyethylene, and the blending ratio is (1:3) to (3:1).

5. The externally-admixed asphalt mixture modifier according to claim 1, characterized in that: The rubber material is thermoplastic elastomer rubber; the anti-stripping agent is an inorganic adhesive; and the cold-resistant agent is automobile lubricating oil or furfural oil.

6. The externally-admixed asphalt mixture modifier according to claim 1, characterized in that: The weathering agent is at least one of an ultraviolet absorber and a light stabilizer.

7. The externally-admixed asphalt mixture modifier according to claim 6, characterized in that: The weathering agent is preferably a mixture of an ultraviolet absorber and a light stabilizer, and the compounding ratio is 1:1; the ultraviolet absorber is a benzotriazole ultraviolet absorber; and the light stabilizer is preferably a hindered amine light stabilizer.

8. The externally-admixed asphalt mixture modifier according to claim 1, characterized in that: The heat-resistant agent is a blend of tris(2,4-di-tert-butylbenzene)phosphite and pentaerythritol tetrakis[β-(3.5-di-tert-butyl-4-hydroxyphenyl)propionate] in a mixing mass ratio of 1:2; the lubricant is any one of ethylene bisstearamide lubricants, polyolefin wax, and stearic acid lubricants.

9. The method for preparing the externally-admixed asphalt mixture modifier according to any one of claims 1 to 8, characterized in that: The following steps are involved: Step 1: Heat the cold-resistant agent to 80℃~100℃; Step 2: Put polyolefin, rubber material, anti-stripping agent, weathering agent, heat-resistant agent and lubricant into a mixing tank in order by weight, then add the cold-resistant agent in step 1, and stir at a stirring speed of 400 to 600 r / min for 2 to 4 minutes to obtain a uniform mixture; Step 3: Add the mixture obtained in step 2 to a twin-screw extruder for plasticization, shearing, and melting to form a uniform melt. The extrusion temperature is set to 120-150°C, the vacuum degree is -0.1-0.04MPa, and the screw speed is set to 350-500r / min. The melt is pulled through the extrusion die, and then cooled, dried, blown dry, and pelletized to obtain modifier particles.

10. Use of the externally-admixed asphalt mixture modifier according to any one of claims 1 to 8 in a dry externally-admixed asphalt mixture.