High-toughness anti-falling polypropylene composite material as well as preparation method and application thereof
By combining maleic anhydride grafted elastomer with epoxy cage polysilsesquioxane and polyamide fiber, a high-tough anti-fall polypropylene composite material is formed, which solves the problem of poor anti-fall performance of polypropylene plastic containers. It has achieved improvements in high strength, modulus and anti-depression performance, especially in low temperatures.
Patent Information
- Application Number
- CN202411148743.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-08-21
AI Technical Summary
Polypropylene plastic containers have poor anti-fall performance, especially at low temperatures, and existing toughening modification methods often sacrifice strength and modulus, and inorganic fiber reinforcement has problems of equipment wear and recycling.
Maleic anhydride grafted elastomer and epoxy-based cage polysilsesquioxane to form core-shell structure particles, and combined with polyamide fibers through in-situ fiberization technology to form a high-tough anti-fall polypropylene composite material, through the interface Graft copolymerization and fiber bridging improve toughness and modulus, while using curing accelerators to freeze the fiber state in subsequent processing to avoid fiber recovery.
It significantly improves the impact resistance and tensile strength of polypropylene composite materials, maintains high strength and modulus, improves the compatibility of polyamide fibers and polypropylene, and improves the anti-drop performance of plastic containers, especially at low temperatures. rupture.
Smart Images

Figure BDA0005002984310000021 
Figure BDA0005002984310000022 
Figure BDA0005002984310000061
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of plastic packaging, and more specifically, relates to a high-toughness, drop-resistant polypropylene composite material and a preparation method and application thereof. Background Art
[0002] Polypropylene (PP), as the lightest general-purpose plastic, has the advantages of being easy to process, low in price, non-toxic and tasteless, and is widely used in daily life. However, PP has poor toughness, is brittle at low temperatures, and has low impact strength. PP plastic containers made from it, especially thin-walled plastic containers, have poor drop resistance and are easily broken, which limits their scope of application. Therefore, the toughening and modification of PP has always been a hot topic of research. Among them, blending modification is the mainstream method for PP toughening and modification because of its significant effect, low cost, fast operation, and can be quickly transformed into industrial applications.
[0003] The impact toughness of PP can be improved by adding elastomers such as rubber and thermoplastic elastomers. The elastomer content, dispersion form, and compatibility with the matrix will affect the toughening effect of PP. However, the improvement of the toughness of elastomer-modified PP often comes at the expense of strength and modulus: in order to fully improve the toughness of PP, a higher content of elastomer needs to be added, which will inevitably significantly reduce the rigidity and tensile strength of the modified PP system.
[0004] In order to make up for the strength and modulus lost by adding elastomers, high-strength materials such as glass fiber and carbon fiber can be added to improve the tensile strength and elastic modulus of PP, but such inorganic fibers will increase the viscosity of the system, cause large equipment wear, and be difficult to recycle; another method is to change the processing conditions and adjust the morphology of the dispersed phase in the continuous phase of the two-phase blend to improve the performance of the polymer material, such as using the polymer in-situ fiberization method to prepare an in-situ fiberization blending system, such as patent CN110423403A. Compared with traditional inorganic fiber reinforcement, the microfibers formed by in-situ fiberization have the advantages of uniform dispersion, obvious and controllable reinforcement effect, and recyclability.
[0005] However, the fiber morphology of in-situ fiberization is metastable in nature and needs to be carefully preserved during post-processing. It needs to be reprocessed at a temperature below the melting point of the dispersed phase to prevent the microfibers from returning to a spherical state, so the post-processing process is limited. In addition, studies have shown that for in-situ fiberization technology, when no or only a small amount of compatibilizer is added, the two phases of the blend are weakly compatible, which is conducive to the deformation and slippage of the dispersed phase in the matrix, thereby forming microfibers; adding more compatibilizers will lead to a decrease in the aspect ratio of the microfibers and an uneven diameter distribution, making the toughening and strengthening effect on PP not obvious. However, when no or only a small amount of compatibilizer is added, the compatibility between the formed microfibers and the matrix is poor, forming more voids, and the weak interfacial bonding not only affects the stress transfer of the two phases, but its interface defects will also form a large number of stress concentration points, resulting in a decrease in mechanical properties. Summary of the invention
[0006] The purpose of the present invention is to overcome the deficiencies of the prior art and provide a high-toughness and drop-resistant polypropylene composite material, which has high notched impact strength, high flexural modulus, high tensile strength and good drop resistance, and is particularly suitable for preparing polypropylene plastic containers.
[0007] Another object of the present invention is to provide a method for preparing the above-mentioned high-toughness and drop-resistant polypropylene composite material.
[0008] Another object of the present invention is to provide the use of the above-mentioned high-toughness and drop-resistant polypropylene composite material in the preparation of plastic containers.
[0009] In order to solve the above technical problems, the technical solution adopted by the present invention is:
[0010] A high-toughness, drop-resistant polypropylene composite material comprises the following components in parts by weight:
[0011]
[0012] The polypropylene-polyamide in-situ fiber-forming composite material comprises the following components in parts by weight:
[0013]
[0014] The present invention toughens and modifies polypropylene by maleic anhydride grafted elastomer, and adds epoxy cage-type polysilsesquioxane (G-POSS) to form hard-core soft-shell structure particles with G-POSS as the core and maleic anhydride grafted elastomer as the shell. In the high-temperature melting process, the epoxy group of G-POSS can react with the maleic anhydride group of the maleic anhydride grafted elastomer, so that graft copolymerization occurs at the interface, forming more entanglements and higher molecular weight; and the special organic-inorganic hybrid structure of G-POSS can also provide certain mechanical strength, and is conducive to reducing the dispersed phase particle size, and the multi-faceted coordination enables the strength and modulus of the composite material to be maintained. When the core-shell particles are impacted, multiple cavities are formed at the interface or inside thereof, thereby absorbing a large amount of energy, and the tip stress of crack extension is absorbed and buffered by the elastomer particles, the crack extension is blocked, and the impact resistance is improved.
[0015] The present invention also adopts in-situ fibrillation to obtain a polypropylene-polyamide in-situ fiber-forming composite material, and in the presence of a curing accelerator, utilizes a cross-linking reaction between an epoxy cross-linking agent and an amine group to freeze the fiber state of the polyamide, so that it will not recover to a spherical state in subsequent high temperature (280-300°C) processing. Polyamide has the advantages of high strength, good rigidity, and impact resistance. The fibers formed form a mutually entangled network structure in the polypropylene matrix, and consume energy through the bridging effect and pull-out effect of the fibers, thereby inhibiting the expansion of cracks, significantly improving the toughness of the system, and improving the rigidity of the matrix. The present invention does not add or only adds a small amount of a compatibilizer during the in-situ fibrillation process, which is conducive to the formation of a polypropylene-polyamide in-situ fiber-forming composite material containing microfibers with a large aspect ratio. When blended with polypropylene, maleic anhydride grafted elastomer, etc., the maleic anhydride grafted elastomer not only reacts with the epoxy group to be coated on G-POSS, but is also partially distributed on the surface of the PA fiber, increasing the compatibility of the PA fiber and PP, solving the interface defects caused by the weak interface bonding between the PA fiber and PP, and thus improving the mechanical properties.
[0016] Preferably, the polypropylene has a melt flow rate of 10 to 50 g / 10 min measured at 230° C. and 2.16 kg.
[0017] Preferably, the maleic anhydride grafted elastomer is a mixture of one or more of maleic anhydride grafted ethylene-octene copolymer (MAH-POE), maleic anhydride grafted ethylene propylene rubber (MAH-EPDM), maleic anhydride grafted ethylene-propylene copolymer (MAH-EPR), maleic anhydride grafted ethylene-butene copolymer (MAH-EBR), maleic anhydride grafted styrene-ethylene-butadiene-styrene block copolymer (MAH-SEBS), and maleic anhydride grafted ethylene-vinyl acetate rubber (MAH-EVA).
[0018] Preferably, the maleic anhydride grafting rate of the maleic anhydride grafted elastomer is 1 to 5 wt%.
[0019] Preferably, each molecule of the epoxy cage-type polysilsesquioxane contains 8 epoxy groups.
[0020] Preferably, the epoxy cage-type polysilsesquioxane is one or a mixture of two of epoxycyclohexyl-cage polysilsesquioxane and glycidyloxypropyl-cage polysilsesquioxane.
[0021] Preferably, the polyamide is a mixture of one or more of polycaprolactam (PA6), polyhexamethylene adipamide (PA66), polypentamethylene adipamide (PA56), and polydecanediamine sebacate (PA1010).
[0022] Preferably, the polyamide has a melt flow rate of 1 to 30 g / 10 min measured at 230° C. and 2.16 kg.
[0023] Preferably, the compatibilizer is one or a blend of two of maleic anhydride grafted polyolefin and glycidyl methacrylate grafted polyolefin.
[0024] More preferably, the maleic anhydride grafting rate of the maleic anhydride grafted polyolefin is 1 to 5 wt %.
[0025] More preferably, the glycidyl methacrylate grafting rate of the glycidyl methacrylate grafted polyolefin is 1 to 5 wt %.
[0026] Further preferably, the maleic anhydride grafted polyolefin is a mixture of one or more of maleic anhydride grafted polypropylene (MAH-PP), maleic anhydride grafted polyethylene (MAH-PE), maleic anhydride grafted ethylene-octene copolymer (MAH-POE), maleic anhydride grafted ethylene-propylene copolymer (MAH-EPR), and maleic anhydride grafted ethylene-butene copolymer (MAH-EBR); the glycidyl methacrylate grafted polyolefin is a mixture of one or more of glycidyl methacrylate grafted polypropylene (GMA-PP), glycidyl methacrylate grafted polyethylene (GMA-PE), and glycidyl methacrylate grafted ethylene-octene copolymer (GMA-POE).
[0027] Preferably, the epoxy crosslinking agent is ethylene glycol glycidyl ether, diethylene glycol glycidyl ether or a mixture of both.
[0028] Preferably, the curing accelerator is a mixture of one or more of phenol, 2,4,6-tris(dimethylaminomethyl)phenol, triethanolamine, N,N-dimethylethanolamine and benzyl alcohol.
[0029] Preferably, the method for preparing the polypropylene-polyamide in-situ fiber-forming composite material comprises the following steps:
[0030] S01, fully stirring and mixing polyamide, epoxy crosslinking agent and curing accelerator, and then uniformly mixing with compatibilizer and polypropylene to obtain a premix;
[0031] S02, adding the premix of step S01 into a twin-screw extruder, and subjecting the premix to melt extrusion-heat stretching-quenching-granulation to obtain in-situ fibrillated plastic pellets; the temperature of the twin-screw extruder is set to 210-240° C., the screw speed is 100-250 r / min, and the traction roller motor speed is 50-70 r / min;
[0032] S03, placing the plastic pellets in step S02 in an oven at 100-130°C for 8-12 hours to obtain the polypropylene-polyamide in-situ fiber-forming composite material.
[0033] The preparation method of the above-mentioned high-toughness and drop-resistant polypropylene composite material comprises the following steps:
[0034] S11. The polypropylene - polyamide in-situ fiber composite material, polypropylene, maleic anhydride grafted elastomer, epoxy cage polysilsesquioxane was added to the mixer and stirred to obtain a mixed material;
[0035] S12. The mixed material in S11 is extruded and granulated using a twin-screw extruder to obtain a high-toughness and drop-resistant polypropylene composite material.
[0036] Preferably, the temperature of the twin-screw extruder is set to 280-300° C., and the screw speed of the twin-screw extruder is 100-500 rpm.
[0037] The application of the above-mentioned high-toughness and drop-resistant polypropylene composite material in plastic containers also falls within the protection scope of the present invention.
[0038] The high-toughness and drop-resistant polypropylene composite material is prepared through injection molding, stretching and blow molding to obtain the plastic container.
[0039] Compared with the prior art, the present invention has the following beneficial effects:
[0040] The present invention adopts core-shell structure particles with POSS as core and elastomer as shell and polyamide fiber to synergistically toughen and strengthen polypropylene. When impacted, multiple cavities are formed at the interface or inside of the core-shell particles, thereby absorbing a large amount of energy, and the tip stress of crack propagation is absorbed and buffered by the elastomer particles, crack propagation is hindered, and the impact resistance of the material is improved. At the same time, the strength and modulus of the high-toughness anti-fall polypropylene composite material are maintained at a high level. On the other hand, polyamide fiber consumes energy through the bridging effect and pull-out effect of the fiber, thereby suppressing the expansion of cracks, and the high specific surface area of the fiber itself and the network structure formed by mutual entanglement also improve the toughness and tensile strength of the composite material.
[0041] The present invention does not add or only adds a small amount of compatibilizer during the in-situ fiber forming process, forms polyamide microfibers with a large aspect ratio, and freezes the fiber state of the polyamide through a crosslinking agent in the presence of a curing accelerator. In subsequent processing, the maleic anhydride grafted elastomer is distributed on the surface of the polyamide fiber, which enhances the compatibility of the polyamide fiber and polypropylene, so that the composite material can obtain fibers with a large aspect ratio and solve the weak interface bonding between the PA fiber and the PP during in-situ fiber forming.
[0042] The polypropylene plastic made from the high-toughness and drop-resistant polypropylene composite material of the invention has good toughness, high impact strength and good tensile performance. The made plastic container has excellent drop resistance, especially drop resistance at low temperatures, and the plastic container does not crack at low temperatures. DETAILED DESCRIPTION
[0043] The present invention is further described below in conjunction with specific examples, but the examples do not limit the present invention in any form. Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art. Unless otherwise specified, the reagents and materials used in the present invention are commercially available.
[0044] The following raw materials were used in the examples and comparative examples of the present invention:
[0045] Polypropylene (PP): PP Z30S, LyondellBasell Industries;
[0046] Polyhexamethylene adipamide (PA66): FYR27, Henan Shenma Nylon Chemical Co., Ltd.;
[0047] Polycaprolactam (PA6): 1013B, Japan Ube Co., Ltd.;
[0048] Glycidyloxypropyl-cage polysilsesquioxane (G-POSS): Xi'an Qiyue Biotechnology Co., Ltd.;
[0049] Ethylene-octene copolymer (POE): DF710, Mitsui Chemicals, Japan;
[0050] Maleic anhydride grafted ethylene-octene copolymer (MAH-POE): homemade, the process is as follows:
[0051] Weigh 100 parts by weight of POE (Mitsui Chemicals DF710, Japan) and 500 parts by weight of toluene in a reactor and heat to dissolve; add 4 parts by weight of MAH and 4 parts by weight of diisopropylbenzene peroxide, stir and react at 150°C for 5 hours, and filter out toluene; wash with ethanol 4 to 6 times to wash away unreacted MAH; and vacuum dry to obtain MAH-POE with a grafting rate of 1.3%.
[0052] Maleic anhydride grafted ethylene propylene diene monomer rubber (MAH-EPDM): SWR-3F1, Dongguan Jingke Polymer Co., Ltd.;
[0053] Glycidyl methacrylate grafted ethylene-octene copolymer (GMA-POE): homemade, the process is as follows: weigh 100 parts by weight of POE (Japan Mitsui Chemicals DF710), 5 parts by weight of GMA, 0.5 parts by weight of diisopropylbenzene peroxide, mix evenly, control the temperature of the internal mixer to 165°C, the speed to 30r / min, mix for 8 minutes, and chop the product into particles. At 80°C, dissolve the product in xylene, heat and reflux for 4 hours, pour acetone into the solution while hot and use a Buchner funnel to reduce pressure and filter, repeat twice to remove impurities such as unreacted GMA and homopolymerized GMA; vacuum dry, the resulting GMA-POE has a grafting rate of 1.3%.
[0054] Maleic anhydride grafted polypropylene (MAH-PP): XYJ1210, Dongguan Xingyuan Chemical Co., Ltd.;
[0055] Octamethyl caged polysilsesquioxane: Xi'an Qiyue Biotechnology Co., Ltd.
[0056] The polypropylene-polyamide in-situ fiber-forming composite material is homemade, and the formula and preparation method are as follows:
[0057] Table 1 (raw material addition amount, unit: weight part)
[0058]
[0059]
[0060] Preparation of PP / PA-1 and PP / PA-2:
[0061] 1) fully stirring and mixing polyhexamethylene adipamide, diethylene glycol glycidyl ether and 2,4,6-tris(dimethylaminomethyl)phenol, and then uniformly mixing with polypropylene and glycidyl methacrylate grafted ethylene-octene copolymer (if any) to obtain a premix;
[0062] 2) adding the premix of step 1) into a twin-screw extruder, and subjecting the premix to melt extrusion-heat stretching-quenching-granulation to obtain in-situ fibrillated plastic pellets; the temperature of the twin-screw extruder is set at 210-240° C., the screw speed is 100-250 r / min, and the traction roller motor speed is 50 r / min;
[0063] 3) placing the plastic pellets from step 2) in an oven at 130° C. for 8 hours to obtain the polypropylene-polyamide in-situ fiber-forming composite material.
[0064] Preparation of PP / PA-3 and PP / PA-4:
[0065] 1) fully stirring and mixing polycaprolactam, diethylene glycol glycidyl ether and 2,4,6-tris(dimethylaminomethyl)phenol, and then uniformly mixing with polypropylene and maleic anhydride grafted polypropylene to obtain a premix;
[0066] 2) adding the premix of step 1) into a twin-screw extruder, and subjecting the premix to melt extrusion-heat stretching-quenching-granulation to obtain in-situ fibrillated plastic pellets; the temperature of the twin-screw extruder is set at 210-230° C., the screw speed is 100-250 r / min, and the traction roller motor speed is 70 r / min;
[0067] 3) placing the plastic pellets from step 2) in an oven at 100° C. for 12 hours to obtain the polypropylene-polyamide in-situ fiber-forming composite material.
[0068] Preparation of PP / PA-5:
[0069] 1) fully stirring and mixing polyhexamethylene adipamide and 2,4,6-tris(dimethylaminomethyl)phenol, and then uniformly mixing with polypropylene and glycidyl methacrylate grafted ethylene-octene copolymer to obtain a premix;
[0070] 2) adding the premix of step 1) into a twin-screw extruder, and obtaining in-situ fibrillated plastic pellets through melt extrusion-heat stretching-quenching-pelletizing; the temperature of the twin-screw extruder is set to 210-240° C., the screw speed is 100-250 r / min, and the traction roller motor speed is 50 r / min.
[0071] 3) placing the plastic pellets from step 2) in an oven at 130° C. for 8 hours to obtain the polypropylene-polyamide in-situ fiber-forming composite material.
[0072] Preparation of PP / PA-6:
[0073] 1) fully stirring and mixing polyhexamethylene adipamide and diethylene glycol glycidyl ether, and then uniformly mixing with polypropylene and glycidyl methacrylate grafted ethylene-octene copolymer to obtain a premix;
[0074] 2) adding the premix of step 1) into a twin-screw extruder, and subjecting the premix to melt extrusion-heat stretching-quenching-granulation to obtain in-situ fibrillated plastic pellets; the temperature of the twin-screw extruder is set at 210-240° C., the screw speed is 100-250 r / min, and the traction roller motor speed is 50 r / min;
[0075] 3) placing the plastic pellets from step 2) in an oven at 130° C. for 8 hours to obtain the polypropylene-polyamide in-situ fiber-forming composite material.
[0076] Embodiments 1 to 4
[0077] Examples 1 to 4 provide a series of high-toughness, drop-resistant polypropylene composite materials, which are prepared according to the formulation in Table 2 and the following steps.
[0078] S1. The polypropylene-polyamide in-situ fiber-forming composite material, polypropylene (if any), maleic anhydride grafted elastomer, epoxy cage polysilsesquioxane were added into a mixer and stirred to obtain a mixed material;
[0079] S2. The mixed material in S1 is extruded and granulated by a twin-screw extruder to obtain a high-toughness and drop-resistant polypropylene composite material. The temperature of the twin-screw extruder is set to 280-300° C., and the screw speed of the twin-screw extruder is 100-500 rpm.
[0080] Table 2 Formula of Examples 1 to 4 (raw material addition amount, unit: weight parts)
[0081]
[0082]
[0083] Comparative Examples 1 to 6
[0084] Comparative Examples 1 to 6 provide a series of polypropylene composite materials, the formulations are shown in Table 3, and the preparation methods are the same as those of Example 1.
[0085] Table 3 (raw material addition amount, unit: weight parts)
[0086]
[0087] The performance of the polypropylene composite materials prepared in the above examples and comparative examples was tested.
[0088] 1. Tensile properties: The tensile strength of polypropylene composites was determined according to ASTM D638.
[0089] 2. Flexural modulus: The flexural modulus of polypropylene composites was measured according to ASTM D790.
[0090] 3. Impact strength: The Izod notched impact strength of polypropylene composites was measured according to ASTM D256.
[0091] 4. Drop resistance: The polypropylene composite material was made into a plastic bottle with a size of 100 ml and a wall thickness of 0.6±0.1 mm. The drop resistance was tested in accordance with YBB00102002-2015. The test conditions were: the drop resistance was tested at 25°C and -30°C, 1.5m high, and the damage of the plastic bottle was observed after falling 3 times.
[0092] Performance Test Results
[0093] The performance test results of the polypropylene composite materials and PP plastic bottles of Examples 1 to 4 and Comparative Examples 1 to 6 are shown in Table 3.
[0094] PP Z30S polypropylene has a tensile strength of 34.3MPa, a flexural modulus of 1470MPa, and an Izod notched impact strength of 20J / m.
[0095] Table 4
[0096]
[0097] It can be seen from Table 3 that the tensile strength of the polypropylene composite materials in Examples 1 to 4 is all above 52 MPa, the flexural modulus is all above 1950 MPa, the impact strength is all above 52 J / m, and the plastic bottles are not broken in the drop resistance tests at 25°C and -30°C, which shows that the polypropylene composite materials of the present invention have excellent tensile strength, flexural modulus and impact strength, and excellent drop resistance at room temperature and low temperature.
[0098] It can be seen from Example 2 and Comparative Example 1 that in the process of in-situ fiberization of polypropylene-polyamide, when no epoxy crosslinking agent is used for crosslinking, the tensile strength, flexural modulus and notched impact strength of the prepared polypropylene composite material are significantly reduced, and the plastic bottle is broken in the -30°C low temperature drop resistance test. This is because the uncrosslinked and cured polyamide fibers return to a spherical state at a processing temperature of 280 to 300°C in the subsequent preparation of the polypropylene composite material.
[0099] It can be seen from Example 2 and Comparative Example 2 that in the process of in-situ fiberization of polypropylene-polyamide, when no curing accelerator is used, the tensile strength and notched impact strength of the prepared polypropylene composite material are significantly reduced, the flexural modulus is reduced, and the plastic bottle has cracks in the -30°C low temperature drop resistance test. This is because there is no curing accelerator to promote cross-linking, so that the cross-linking degree of the polyamide fiber is low, and it is difficult to maintain a complete fiber state at the processing temperature of 280-300°C in the subsequent preparation of the polypropylene composite material.
[0100] It can be seen from Example 2 and Comparative Example 3 that when the epoxy cage-like polysilsesquioxane is not used in the polypropylene composite material, the flexural modulus of the polypropylene composite material decreases, and the tensile strength and notched impact strength decrease significantly. The plastic bottle has cracks in the -30°C low-temperature drop resistance test. It can be seen that the use of G-POSS has an effect on the improvement of flexural modulus, tensile strength and impact strength.
[0101] As shown in Example 2 and Comparative Example 4, ethylene-octene copolymer is used to replace maleic anhydride grafted ethylene-octene copolymer, and the tensile strength, flexural modulus and notched impact strength of the prepared polypropylene composite material are all significantly reduced, and the plastic bottle is broken in the -30°C low temperature drop resistance test. This is because polypropylene and ethylene-octene copolymer are both non-polar materials, and G-POSS is a polar material, and the ethylene-octene copolymer without grafted maleic anhydride group can neither react with G-POSS, and is difficult to coat G-POSS to form a core-shell structure, nor can it be used as a compatibilizer to improve the compatibility of polyamide fiber and polypropylene; and polar G-POSS has poor compatibility with the system, and defects can be formed instead, resulting in the mechanical properties of polypropylene composite materials, especially the deterioration of impact strength.
[0102] It can be seen from Example 2 and Comparative Example 5 that when glycidyl methacrylate grafted ethylene-octene copolymer is used instead of maleic anhydride grafted ethylene-octene copolymer, under the action of interfacial tension, GMA-POE can still coat G-POSS to form a core-shell structure, but no graft copolymerization occurs between the two, and more entanglements and higher molecular weight cannot be formed, resulting in the mechanical properties of the prepared polypropylene composite material not being significantly improved, and the plastic bottle has cracks in the -30°C low temperature drop resistance test.
[0103] It can be seen from Example 2 and Comparative Example 6 that when octamethyl caged polysilsesquioxane is used to replace epoxy caged polysilsesquioxane, the tensile strength and notched impact strength of the prepared polypropylene composite material are significantly reduced, the flexural modulus is reduced, and the plastic bottle has cracks in the -30°C low temperature drop resistance test. This is because octamethyl POSS has no reactive epoxy group and has low polarity, and can neither react with MAH-POE nor form a core-shell structure with MAH-POE under the action of interfacial tension. Combined with Comparative Example 3, it can be seen that its addition has little effect on improving the mechanical properties of the polypropylene composite material.
[0104] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not intended to limit the embodiments of the present invention. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the embodiments here. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the claims of the present invention.
Claims
1. A high-toughness, drop-resistant polypropylene composite material, characterized in that: The high-toughness, drop-resistant polypropylene composite material comprises the following components in parts by mass: The polypropylene-polyamide in-situ fiber-forming composite material comprises the following components in parts by weight:
2. The high-toughness, drop-resistant polypropylene composite material according to claim 1, characterized in that: The maleic anhydride grafted elastomer is a mixture of one or more of maleic anhydride grafted ethylene-octene copolymer, maleic anhydride grafted ethylene-propylene copolymer, maleic anhydride grafted ethylene-butylene copolymer, maleic anhydride grafted styrene-ethylene-butadiene-styrene block copolymer, and maleic anhydride grafted ethylene-vinyl acetate rubber.
3. The high-toughness and drop-resistant polypropylene composite material according to claim 1, characterized in that: The epoxy cage-type polysilsesquioxane is one or a mixture of two of epoxycyclohexyl-cage-type polysilsesquioxane and glycidyloxypropyl-cage-type polysilsesquioxane.
4. The high-toughness, drop-resistant polypropylene composite material according to claim 1, characterized in that: The polyamide is a mixture of one or more of polycaprolactam, polyhexamethylene adipamide, polypentamethylene adipamide and polydecamethylene sebacamide.
5. The high-toughness, drop-resistant polypropylene composite material according to claim 1, characterized in that: The compatibilizer is one or a blend of two of maleic anhydride grafted polyolefin and glycidyl methacrylate grafted polyolefin.
6. The high-toughness, drop-resistant polypropylene composite material according to claim 1, characterized in that: The epoxy crosslinking agent is one of ethylene glycol glycidyl ether and diethylene glycol glycidyl ether or a mixture of the two.
7. The high-toughness, drop-resistant polypropylene composite material according to claim 1, characterized in that: The curing accelerator is a mixture of one or more of phenol, 2,4,6-tris(dimethylaminomethyl)phenol, triethanolamine, N,N-dimethylethanolamine and benzyl alcohol.
8. The high-toughness, drop-resistant polypropylene composite material according to any one of claims 1 to 7, characterized in that: The preparation method of the polypropylene-polyamide in-situ fiber-forming composite material comprises the following steps: S01, fully stirring and mixing polyamide, epoxy crosslinking agent and curing accelerator, and then uniformly mixing with compatibilizer and polypropylene to obtain a premix; S02, adding the premix of step S01 into a twin-screw extruder, and obtaining in-situ fibrillated plastic pellets through melt extrusion-hot stretching-quenching-granulation; the temperature of the twin-screw extruder is set to 210-240° C., the screw speed is 100-300 r / min, and the traction roller motor speed is 50-70 r / min; S03, placing the plastic pellets in step S02 in an oven at 100-130°C for 8-12 hours to obtain the polypropylene-polyamide in-situ fiber-forming composite material.
9. The method for preparing the high-toughness and drop-resistant polypropylene composite material according to any one of claims 1 to 8, characterized in that: The steps include: S11. The polypropylene / polyamide in-situ fiber composite material, polypropylene, maleic anhydride grafted elastomer, epoxy cage polysilsesquioxane was added to a mixer and stirred to obtain a mixed material; S12. The mixed material in S11 is extruded and granulated by a twin-screw extruder to obtain a high-toughness and drop-resistant polypropylene composite material. The temperature of the twin-screw extruder is set to 280-300° C., and the screw speed of the twin-screw extruder is 100-500 rpm.
10. Use of the high-toughness, drop-resistant polypropylene composite material according to any one of claims 1 to 8 in plastic containers.
Citation Information
Patent Citations
Preparation method for maleic anhydride grafting modified carbon fiber / polyamide / polypropylene composite material
CN101544822A
Superparamagnetic nano micelle containing POSS (polyhedral oligomeric silsesquioxane) and preparation method thereof
CN103709715A
Halogen-free flame-retarding polyamide material and preparation method thereof
CN109370207A
Composite in-situ fiber-forming reinforced polymer material and preparation method and device thereof
CN110423403A
Reinforced toughened polypropylene material preparing method
CN1472246A
Cited By
High-toughness polypropylene suction nozzle tube and preparation method thereof
CN121628274A