High-strength high-slippage glass fiber reinforced CPVC (chlorinated polyvinyl chloride) material and preparation method thereof
By using hyperbranched polar alkyl polyester and polydimethylsiloxane in CPVC materials, the dispersion and wettability of glass fiber are improved, and the low strength and surface floating of glass fiber reinforced CPVC materials are solved. The fiber problem has achieved high strength, low friction and good processing performance materials, suitable for high strength, low friction pipes and special profile fields.
Patent Information
- Application Number
- CN202411150779.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-08
AI Technical Summary
The existing glass fiber reinforced CPVC materials have low strength and severe surface floating fibers, resulting in difficulty in processing and forming and limited application range.
Hyperbranched polar alkyl polyester as compatibilizer and polydimethylsiloxane as slip agent, combined with other additives to improve the dispersion and wetting of glass fiber in CPVC, and enhance the material mechanical properties and surface smoothness.
Achieve high-strength and low-friction glass fiber reinforced CPVC material, with tensile strength of more than 75MPa, bending modulus exceeding 11000MPa, surface friction coefficient is less than 0.2, and dynamic stability time exceeding 1400s. It is suitable for high-strength, low-friction pipes and special profile fields. Application.
Smart Images

Figure CN118909371A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polymer materials, and in particular relates to a high-strength and high-slip glass fiber reinforced CPVC material and a preparation method thereof. Background Art
[0002] Chlorinated polyvinyl chloride resin (CPVC) is a product obtained by further chlorination modification of polyvinyl chloride resin. It is a new type of engineering plastic. Its mass content of chlorine is usually in the range of 62% to 69%. It has excellent flame retardancy, heat resistance, weather resistance, etc. It can be used for fire protection pipes, chemical pipes, power pipes and brackets. After adding glass fiber reinforcement, the tensile strength is greatly improved, and the bending modulus is greatly improved, making the downstream products high in strength, heavy in load bearing, and more durable. However, CPVC has high viscosity and is not easy to process; after adding glass fiber, due to the high viscosity of the matrix resin, the glass fiber is not well dispersed, the strength is not improved much, and the floating fiber seriously limits the application range of CPVC.
[0003] At present, in glass fiber reinforced materials, the main additives to improve the dispersion of glass fiber are modified wax additives containing polar groups, such as TAF. With ethylene bis fatty acid amide (EBS) as the base material, reactive monomers containing polar groups react with EBS under the action of catalysts to form BAB type copolymers; the slip additives to improve the surface of CPVC mainly include fluorine-containing compounds and ultra-high molecular weight silicon-containing compounds such as polytetrafluoroethylene and silicone masterbatch; but CPVC has high viscosity and low processing temperature. Such additives are poorly dispersed at the processing temperature of CPVC, so the dispersion and wetting effect on glass fiber in CPVC is very poor, resulting in low strength of the material and severe surface roughness of floating fibers.
[0004] CN116769261A discloses a PVC / CPVC / ABS alloy composite material, which is composed of the following formula, which is calculated by weight: polyvinyl chloride resin 50-100, chlorinated polyvinyl chloride resin 50-75, acrylonitrile-butadiene-styrene terpolymer resin 5-30, filler 5-30, coupling agent 0.1-0.8, stabilizer 3.0-8.0, processing aid 1.0-6.0, anti-impact agent 3-12, antioxidant 0.1-1.0, pigment 0.01-0.05, light stabilizer 0.1-1.2, lubricant 0.3-1.2, and is intended to solve the problems that the power pipes produced by the current formula often cannot meet the requirements of industry quality standards, the Vicat softening temperature is low, the impact performance is poor, and the processing and molding difficulties caused by poor fluidity. However, the defects of this technology are low strength, low Vicat softening temperature, and harsh processing conditions caused by a large number of alloy materials.
[0005] Therefore, how to overcome the defects of existing glass fiber reinforced CPVC materials such as low strength and severe surface floating fibers is a technical problem that needs to be solved urgently. Summary of the invention
[0006] In order to solve the problems of the prior art, the present invention provides a high-strength and high-slip glass fiber reinforced CPVC material. The present invention uses hyperbranched polar alkyl polyester as a compatibilizer, polydimethylsiloxane as a slip agent, and other additives to synergistically compound to obtain a high-strength and high-slip glass fiber reinforced CPVC material, which solves the problem that the current CPVC has poor glass fiber dispersion due to its high viscosity, which leads to poor mechanical strength of the material, rough surface and high friction.
[0007] The technical solution of the present invention is as follows:
[0008] A high-strength and high-slip glass fiber reinforced CPVC material, comprising the following components in parts by weight:
[0009] 60-80 parts of CPVC resin;
[0010] Glass fiber 20-40 parts;
[0011] 5-15 parts of toughening agent;
[0012] Compatibilizer 0.5-2 parts;
[0013] 2-6 parts of slip agent;
[0014] 2-4 parts of stabilizer;
[0015] Antioxidant 0.1-0.5 parts;
[0016] Lubricant 0.5-2 parts;
[0017] 1-2 parts of processing aid;
[0018] The glass fiber reinforced CPVC material has a tensile strength of 65-80 MPa and an Izod beam notched impact strength of 65-70 J / m.
[0019] Furthermore, the glass fiber reinforced CPVC material has a bending strength of 90-110 MPa, a bending modulus of 8500-11500 MPa, a Vicat softening temperature of 126-130° C. 50N / 50° C., and a friction coefficient of 0.10-0.20.
[0020] Furthermore, the CPVC resin has a degree of polymerization of 650-1050 and contains 66-69% by mass of chlorine.
[0021] Furthermore, the glass fiber is an alkali-free untwisted glass fiber roving, with a fiber diameter of 10-13 μm and a fiber length of 3-5 mm, preferably with a diameter of 13 μm.
[0022] Furthermore, the toughening agent includes at least one of chlorinated polyethylene (CPE), ketone vinyl ester (KEE), and impact-resistant acrylic copolymer (ACR).
[0023] Furthermore, the toughening agent is a compound of CPE and impact-resistant ACR, with a mass ratio of 1:1 to 3:1.
[0024] Furthermore, the compatibilizer is a hyperbranched polar alkyl polyester, which is obtained by modifying the terminal hydroxyl hyperbranched polyester by terminal alkylation with hexadecanoyl chloride, and the terminal hydroxyl hyperbranched polyester has a molecular weight of 6000-9000, a hydroxyl number of 20-30 / mol, and a hydroxyl value of 100-200.
[0025] Furthermore, the preparation method of the hyperbranched polar alkyl polyester is as follows: the terminal hydroxyl hyperbranched polyester is dissolved in tetrahydrofuran, cooled to 0°C in an ice-water bath, and an appropriate amount of triethylamine is added; under nitrogen protection, hexadecanoyl chloride with a molar mass 6 times that of the terminal hydroxyl hyperbranched polyester is added dropwise to the above tetrahydrofuran solution, stirred at 0°C for 1h, and then continued to react at 20°C for 4h. After the reaction is completed, the product is precipitated with water, washed and filtered multiple times, and then dried to obtain a hyperbranched polar alkyl polyester.
[0026] Furthermore, the slip agent is polydimethylsiloxane, and the viscosity at 25°C is ≥30000mm 2 / s.
[0027] Furthermore, the stabilizer is a compound of methyltin mercaptan, pentaerythritol and glycerol, with a mass ratio of 1:0.1:0.4.
[0028] Further, the antioxidant includes at least one of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate (antioxidant 1010), dioctadecyl pentaerythritol bisphosphite (antioxidant 618) or dibenzoylmethane.
[0029] Furthermore, the lubricant includes at least one of polyethylene wax, oxidized polyethylene wax, and C5 / C9 copolymer petroleum resin.
[0030] Further preferably, the lubricant is a compound of polyethylene wax, oxidized polyethylene wax and C5 / C9 copolymer petroleum resin in a mass ratio of 1:1:2.
[0031] Furthermore, the processing aid is an acrylic ester processing aid, which is used to reduce the processing temperature and make the material easier to process.
[0032] The present invention also provides a method for preparing the high-strength and high-slip glass fiber reinforced CPVC material, comprising the following steps:
[0033] Step A) preparing a stabilizer: compounding a stabilizer in a liquid mixer at a temperature of 70-90° C.;
[0034] Step B) Mixing: First, weigh the CPVC resin powder, lubricant, antioxidant, stabilizer, compatibilizer, slip agent, toughening agent and processing aid in parts by weight and put them into a high mixing pot to mix into a premix;
[0035] Step C) extrusion molding: the premix of step B) is added into the twin-screw extruder from the main feed port, the glass fiber is added into the twin-screw extruder from the side feed port, and melt extrusion, drawing and granulation are performed at a temperature of 160-180° C. to obtain the glass fiber reinforced CPVC material.
[0036] Furthermore, in step A), propylene glycol is first added to a liquid mixer, stirred at a low speed and heated to 80° C., then pentaerythritol is added, the heating is stopped and stirring is continued until the pentaerythritol is completely dissolved, and methyltin mercaptan is added, and stirring is continued for 2 minutes until the mixture is evenly stirred to obtain the stabilizer.
[0037] Furthermore, in step A), the rate of the low-speed stirring is 100 rpm.
[0038] Further, in step B), first, CPVC resin powder, lubricant and antioxidant are added to a high mixing pot and mixed at a stirring rate of 100-200 rpm for 1-5 minutes, then a stabilizer is added and mixed at a stirring rate of 300-400 rpm for 1-5 minutes, then a compatibilizer and a slip agent are added and mixed for 1-5 minutes, and finally a toughening agent and a processing aid are added and mixed for 1-5 minutes. When all materials are mixed evenly, mixing is stopped, and the premix is discharged into a storage tank for standby use.
[0039] Furthermore, in step C), the temperature before the side feeding port is 160-180°C, and the temperature after the side feeding port is 160-170°C.
[0040] Further, in step C), the twin-screw extruder includes a plurality of heating sections, and the temperature of each heating section can be set independently. Specifically, the temperature of each zone from the feed port to the discharge port of the twin-screw extruder is set to: 160°C for zone 1 (main feed port), 170°C for zone 2, 175°C for zone 3, 180°C for zone 4, 180°C for zone 5, 180°C for zone 6 (side feed port), 175°C for zone 7, 175°C for zone 8, 175°C for zone 9, 170°C for zone 10, 170°C for zone 11, and 180°C for the die head.
[0041] Furthermore, in step C), the screw length-to-diameter ratio of the twin-screw extruder is 48:1.
[0042] Furthermore, in step C), the particle size of the glass fiber reinforced CPVC material is 2-3 mm.
[0043] The present invention has the following beneficial effects:
[0044] (1) Compared with the existing glass fiber reinforced CPVC material, the glass fiber reinforced CPVC material provided by the present invention, which is prepared by using hyperbranched polar alkyl polyester as a compatibilizer and polydimethylsiloxane as a slip agent, has high strength and a smooth surface and has broad application prospects.
[0045] (2) The compatibilizer hyperbranched polar alkyl polyester of the present invention has a significant effect on the impact strength and rigidity of the glass fiber reinforced CPVC material, and the slip agent polydimethylsiloxane further improves the impact strength and rigidity of the glass fiber reinforced CPVC material. The two work together to make the glass fiber and CPVC resin fully compatible. The tensile strength of the glass fiber reinforced CPVC material finally obtained is up to 75MPa, the bending modulus exceeds 11000MPa, and the cantilever beam notched impact strength exceeds 65J / m. At the same time, the present invention also unexpectedly found that the combined effect of the compatibilizer and the slip agent gives the glass fiber reinforced CPVC material of the present invention a smoother, non-floating fiber surface morphology, and its friction coefficient is less than 0.2.
[0046] (3) In the formulation of the present invention, a stabilizer system of methyl tin mercaptan, pentaerythritol and propylene glycol is used to prepare a glass fiber reinforced CPVC material with a dynamic stability time of more than 1400 seconds, which is 200 seconds longer than that of the traditional organotin and hydrotalcite system, making the material easier to process.
[0047] (4) The present invention obtains a glass fiber reinforced CPVC material with the above-mentioned excellent properties through the innovation of formula composition and preparation process, so it is more suitable for application in the field of high-strength, low-friction pipes and special-shaped materials, replacing traditional metal materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0048] Figure 1 This is a surface morphology diagram of the glass fiber reinforced CPVC material of Example 2 of the present invention.
[0049] Figure 2 This is a surface morphology diagram of the CPVC material of Comparative Example 3 of the present invention.
[0050] Figure 3 This is a SEM electron microscope scanning image of the glass fiber reinforced CPVC material of Example 2 of the present invention.
[0051] Figure 4 This is a SEM electron microscope scanning image of the CPVC material of Comparative Example 3 of the present invention. DETAILED DESCRIPTION
[0052] The preferred embodiments of the present invention will be described in more detail below. Although the preferred embodiments of the present invention are described below, it should be understood that the present invention can be implemented in various forms and should not be limited by the embodiments set forth herein. On the contrary, these embodiments are provided to make the present invention more thorough and complete, and to fully convey the scope of the present invention to those skilled in the art.
[0053] The components used in the embodiments and comparative examples are as follows:
[0054] CPVC resin: H829, purchased from KANEKA, Japan;
[0055] Glass fiber: T635B, purchased from Taishan Glass Fiber Co., Ltd.;
[0056] Toughener I: CPE 135A, purchased from Rizhao Sanxing Chemical Co., Ltd.;
[0057] Toughening agent II: impact-resistant ACR FM-40, purchased from KANEKA, Japan;
[0058] Compatibilizer I: hyperbranched polar alkyl polyester, obtained by alkylating the terminal hydroxyl hyperbranched polyester (HyPerH403, purchased from Wuhan Hyperbranched Resin Technology Co., Ltd.) with hexadecanoyl chloride;
[0059] Compatibilizer II: TR044 (a mixture of fatty acid esters), purchased from Shanghai Zhuangjing Chemical Co., Ltd.;
[0060] Slip agent I: polydimethylsiloxane KF-96H-30000CS, purchased from ShinEtsu Company, Japan;
[0061] Slip agent II: silicone masterbatch and fluoroplastics, silicone masterbatch KJ-A01, purchased from Hangzhou Kaijie Plastic Technology Co., Ltd.; fluoroplastic PTFE, purchased from Guangzhou Energy Innovation Materials Co., Ltd.;
[0062] Stabilizer I: a compound of methyltin mercaptan, pentaerythritol and glycerol, with a mass ratio of 1:0.1:0.4;
[0063] Stabilizer II: a compound of methyltin mercaptan and hydrotalcite, with a mass ratio of 2:1;
[0064] Antioxidant: at least one of antioxidant 1010 and antioxidant 618;
[0065] Lubricant: a compound of polyethylene wax, oxidized polyethylene wax and C5 / C9 copolymer petroleum resin, with a mass ratio of 1:1:2;
[0066] Processing aid: ACR PA-20, purchased from KANEKA, Japan.
[0067] Example 1
[0068] A high-strength and high-slip glass fiber reinforced CPVC material, comprising the following components in parts by weight:
[0069] 75 parts of CPVC resin;
[0070] Glass fiber 25 parts;
[0071] 8 parts of toughening agent;
[0072] Compatilizer I 0.5 part;
[0073] Slip agent 1 3 parts;
[0074] Stabilizer I 3 parts;
[0075] 0.3 parts of antioxidant;
[0076] 2 parts of lubricant;
[0077] 2 parts of processing aid;
[0078] The tensile strength of glass fiber reinforced CPVC material is 69MPa, the flexural strength is 94MPa, the flexural modulus is 8540MPa, the cantilever beam notched impact is 68J / m, the Vicat softening temperature is 126℃, the friction coefficient is 0.13, and the dynamic stability time is 1412s.
[0079] The preparation method is as follows:
[0080] Step A) Preparation of stabilizer I: first, add glycerol into a liquid mixer, stir at a low speed of 100 rpm and heat to 80° C., then add pentaerythritol, stop heating and continue stirring until pentaerythritol is completely dissolved, add methyltin mercaptan, continue stirring for 2 minutes, stir evenly and set aside;
[0081] Step B) Mixing: First, add CPVC resin powder, lubricant and antioxidant into a high mixing pot, mix at 100-200 rpm for 2 minutes, then add stabilizer I and mix at 300-400 rpm for 3 minutes, then add compatibilizer I and slip agent I and mix for 2 minutes, finally add toughening agent and processing aid and mix for 2 minutes, stop mixing when all materials are mixed evenly, and discharge the premix into a storage tank for standby use;
[0082] Step C) extrusion molding: adding the premix of step B) into a twin-screw extruder from a main feed port, adding glass fiber into the twin-screw extruder from a side feed port, and performing melt extrusion, drawing and granulation at a temperature of 160-180° C. to obtain a glass fiber reinforced CPVC material;
[0083] The temperature of each zone from the feed port to the discharge port of the twin-screw extruder is set as follows: zone 1 (main feed port) 160°C, zone 2 170°C, zone 3 175°C, zone 4 180°C, zone 5 180°C, zone 6 (side feed port) 180°C, zone 7 175°C, zone 8 175°C, zone 9 175°C, zone 10 170°C, zone 11 170°C, and die head 180°C; the screw length-diameter ratio of the twin-screw extruder is 48:1,
[0084] Among them, compatibilizer I is prepared by dissolving a terminal hydroxyl hyperbranched polyester in tetrahydrofuran, cooling the mixture to 0°C with an ice-water bath, and adding an appropriate amount of triethylamine; under nitrogen protection, adding hexadecanoyl chloride 6 times the molar mass of the terminal hydroxyl hyperbranched polyester dropwise to the above tetrahydrofuran solution, stirring at 0°C for 1 hour, and then continuing to react at 20°C for 4 hours. After the reaction is completed, the product is precipitated with water, washed and filtered for multiple times, and then dried to obtain compatibilizer I, i.e., a hyperbranched polar alkyl polyester.
[0085] Example 2
[0086] A high-strength and high-slip glass fiber reinforced CPVC material, comprising the following components in parts by weight:
[0087] 65 parts of CPVC resin;
[0088] Glass fiber 35 parts;
[0089] 12 parts of toughening agent;
[0090] 1 part of compatibilizer;
[0091] Slip agent 1 5 parts;
[0092] Stabilizer I 3 parts;
[0093] 0.3 parts of antioxidant;
[0094] 2 parts of lubricant;
[0095] 2 parts of processing aid;
[0096] The tensile strength of glass fiber reinforced CPVC material is 75MPa, the flexural strength is 106MPa, the flexural modulus is 11230MPa, the cantilever beam notched impact is 65J / m, the Vicat softening temperature is 128℃, the friction coefficient is 0.17, and the dynamic stability time is 1457s.
[0097] The preparation method is as follows:
[0098] Step A) Preparation of stabilizer I: first, add glycerol into a liquid mixer, stir at a low speed of 100 rpm and heat to 80° C., then add pentaerythritol, stop heating and continue stirring until pentaerythritol is completely dissolved, add methyltin mercaptan, continue stirring for 2 minutes, stir evenly and set aside;
[0099] Step B) Mixing: First, add CPVC resin powder, lubricant and antioxidant into a high mixing pot, mix at 100-200 rpm for 2 minutes, then add stabilizer I and mix at 300-400 rpm for 3 minutes, then add compatibilizer I and slip agent I and mix for 2 minutes, finally add toughening agent and processing aid and mix for 2 minutes, stop mixing when all materials are mixed evenly, and discharge the premix into a storage tank for standby use;
[0100] Step C) extrusion molding: adding the premix of step B) into a twin-screw extruder from a main feed port, adding glass fiber into the twin-screw extruder from a side feed port, and performing melt extrusion, drawing and granulation at a temperature of 160-180° C. to obtain a glass fiber reinforced CPVC material;
[0101] The temperature of each zone from the feed port to the discharge port of the twin-screw extruder is set as follows: Zone 1 (main feed port) 160°C, Zone 2 170°C, Zone 3 175°C, Zone 4 180°C, Zone 5 180°C, Zone 6 (side feed port) 180°C, Zone 7 175°C, Zone 8 175°C, Zone 9 175°C, Zone 10 170°C, Zone 11 170°C, and the die head is 180°C; the screw length-diameter ratio of the twin-screw extruder is 48:1.
[0102] Among them, compatibilizer I is prepared by dissolving a terminal hydroxyl hyperbranched polyester in tetrahydrofuran, cooling the mixture to 0°C with an ice-water bath, and adding an appropriate amount of triethylamine; under nitrogen protection, adding hexadecanoyl chloride 6 times the molar mass of the terminal hydroxyl hyperbranched polyester dropwise to the above tetrahydrofuran solution, stirring at 0°C for 1 hour, and then continuing to react at 20°C for 4 hours. After the reaction is completed, the product is precipitated with water, washed and filtered for multiple times, and then dried to obtain compatibilizer I, i.e., a hyperbranched polar alkyl polyester.
[0103] Comparative Example 1
[0104] A glass fiber reinforced CPVC material, comprising the following components in parts by weight:
[0105] 75 parts of CPVC resin;
[0106] Glass fiber 25 parts;
[0107] 8 parts of toughening agent;
[0108] Compatibilizer II 0.5 parts;
[0109] Slip agent 1 3 parts;
[0110] Stabilizer I 3 parts;
[0111] 0.3 parts of antioxidant;
[0112] 2 parts of lubricant;
[0113] 2 parts of processing aid;
[0114] The tensile strength of glass fiber reinforced CPVC material is 64MPa, the flexural strength is 86MPa, the flexural modulus is 7920MPa, the cantilever beam notched impact is 59J / m, the Vicat softening temperature is 123℃, the friction coefficient is 1.24, and the dynamic stability time is 1407s.
[0115] The preparation method is as follows:
[0116] Step A) Preparation of stabilizer I: first, add glycerol into a liquid mixer, stir at a low speed of 100 rpm and heat to 80° C., then add pentaerythritol, stop heating and continue stirring until pentaerythritol is completely dissolved, add methyltin mercaptan, continue stirring for 2 minutes, stir evenly and set aside;
[0117] Step B) Mixing: First, add CPVC resin powder, lubricant and antioxidant into a high mixing pot, mix at 100-200 rpm for 2 minutes, then add stabilizer I and mix at 300-400 rpm for 3 minutes, then add compatibilizer II and slip agent I and mix for 2 minutes, finally add toughening agent and processing aid and mix for 2 minutes, stop mixing when all materials are mixed evenly, and discharge the premix into a storage tank for standby use;
[0118] Step C) extrusion molding: adding the premix of step B) into a twin-screw extruder from a main feed port, adding glass fiber into the twin-screw extruder from a side feed port, and performing melt extrusion, drawing and granulation at a temperature of 160-180° C. to obtain a glass fiber reinforced CPVC material;
[0119] The temperatures of each zone from the feed port to the discharge port of the twin-screw extruder are set as follows: zone 1 (main feeding port) 160°C, zone 2 170°C, zone 3 175°C, zone 4 180°C, zone 5 180°C, zone 6 (side feeding port) 180°C, zone 7 175°C, zone 8 175°C, zone 9 175°C, zone 10 170°C, zone 11 170°C, and the die head is 180°C; the screw length-diameter ratio of the twin-screw extruder is 48:1.
[0120] Comparative Example 2
[0121] A glass fiber reinforced CPVC material, comprising the following components in parts by weight:
[0122] 75 parts of CPVC resin;
[0123] Glass fiber 25 parts;
[0124] 8 parts of toughening agent;
[0125] Compatibilizer II 0.5 parts;
[0126] Slip agent II 3.4 parts;
[0127] Stabilizer I 3 parts;
[0128] 0.3 parts of antioxidant;
[0129] 2 parts of lubricant;
[0130] 2 parts of processing aid;
[0131] The tensile strength of glass fiber reinforced CPVC material is 61MPa, the flexural strength is 81MPa, the flexural modulus is 7740MPa, the cantilever beam notched impact is 56J / m, the Vicat softening temperature is 121℃, the friction coefficient is 3.14, and the dynamic stability time is 1425s.
[0132] The preparation method is as follows:
[0133] Step A) Preparation of stabilizer I: first, add glycerol into a liquid mixer, stir at a low speed of 100 rpm and heat to 80° C., then add pentaerythritol, stop heating and continue stirring until pentaerythritol is completely dissolved, add methyltin mercaptan, continue stirring for 2 minutes, stir evenly and set aside;
[0134] Step B) Mixing: First, add CPVC resin powder, lubricant and antioxidant into a high mixing pot, mix at 100-200 rpm for 2 minutes, then add stabilizer I and mix at 300-400 rpm for 3 minutes, then add compatibilizer II and slip agent II and mix for 2 minutes, finally add toughening agent and processing aid and mix for 2 minutes, stop mixing when all materials are mixed evenly, and discharge the premix into a storage tank for standby use;
[0135] Step C) extrusion molding: adding the premix of step B) into a twin-screw extruder from a main feed port, adding glass fiber into the twin-screw extruder from a side feed port, and performing melt extrusion, drawing and granulation at a temperature of 160-180° C. to obtain a glass fiber reinforced CPVC material;
[0136] The temperatures of each zone from the feed port to the discharge port of the twin-screw extruder are set as follows: zone 1 (main feeding port) 160°C, zone 2 170°C, zone 3 175°C, zone 4 180°C, zone 5 180°C, zone 6 (side feeding port) 180°C, zone 7 175°C, zone 8 175°C, zone 9 175°C, zone 10 170°C, zone 11 170°C, and the die head is 180°C; the screw length-diameter ratio of the twin-screw extruder is 48:1.
[0137] Comparative Example 3
[0138] A glass fiber reinforced CPVC material, comprising the following components in parts by weight:
[0139] 75 parts of CPVC resin;
[0140] Glass fiber 25 parts;
[0141] 8 parts of toughening agent;
[0142] Compatibilizer II 1 part;
[0143] Slip agent II 3.4 parts;
[0144] 3 parts of stabilizer II;
[0145] 0.3 parts of antioxidant;
[0146] 2 parts of lubricant;
[0147] 2 parts of processing aid;
[0148] The tensile strength of glass fiber reinforced CPVC material is 58MPa, the flexural strength is 78MPa, the flexural modulus is 7320MPa, the cantilever beam notched impact is 51J / m, the Vicat softening temperature is 121℃, the friction coefficient is 3.25, and the dynamic stability time is 1189s.
[0149] The preparation method is as follows:
[0150] Step A) Preparation of stabilizer II: first, add methyltin mercaptan into a liquid mixer, stir at a low speed of 100 rpm, add hydrotalcite, stir evenly and set aside;
[0151] Step B) Mixing: First, add CPVC resin powder, lubricant and antioxidant into a high mixing pot, mix at 100-200 rpm for 2 minutes, then add stabilizer II and mix at 300-400 rpm for 3 minutes, then add compatibilizer II and slip agent II and mix for 2 minutes, finally add toughening agent and processing aid and mix for 2 minutes, stop mixing when all materials are mixed evenly, and discharge the premix into a storage tank for standby use;
[0152] Step C) extrusion molding: adding the premix of step B) into a twin-screw extruder from a main feed port, adding glass fiber into the twin-screw extruder from a side feed port, and performing melt extrusion, drawing and granulation at a temperature of 160-180° C. to obtain a glass fiber reinforced CPVC material;
[0153] The temperatures of each zone from the feed port to the discharge port of the twin-screw extruder are set as follows: zone 1 (main feeding port) 160°C, zone 2 170°C, zone 3 175°C, zone 4 180°C, zone 5 180°C, zone 6 (side feeding port) 180°C, zone 7 175°C, zone 8 175°C, zone 9 175°C, zone 10 170°C, zone 11 170°C, and the die head is 180°C; the screw length-diameter ratio of the twin-screw extruder is 48:1.
[0154] The formulations of Examples 1-2 and Comparative Examples 1-3 are shown in Table 1.
[0155] Table 1 Formulas of Examples 1-2 and Comparative Examples 1-3
[0156]
[0157] The CPVC materials prepared in Examples 1-2 and Comparative Examples 1-3 were subjected to the performance tests shown in Table 2.
[0158] Table 2 CPVC material properties prepared in Examples 1-2 and Comparative Examples 1-3
[0159]
[0160]
[0161] The performance test results of Examples 1-2 and Comparative Examples 1-3 are shown in Table 2. The results show that the compatibilizer hyperbranched polar alkyl polyester has a very large effect on the rigidity, toughness and surface of the glass fiber reinforced CPVC material, and the slip agent polydimethylsiloxane KF-96H-30000CS has a very large effect on the surface of the glass fiber reinforced CPVC material, and further improves the rigidity and toughness of the glass fiber reinforced CPVC material; hyperbranched polar alkyl polyester as a compatibilizer and polydimethylsiloxane KF-96H-30000CS as a slip agent can prepare a glass fiber reinforced CPVC material with a tensile strength of up to 75 MPa, a flexural modulus of up to 11230 MPa, an impact strength of up to 65 J / m, a Vicat softening temperature of up to 128°C, and a friction coefficient of less than 0.2, which solves the technical problem that the glass fiber reinforced CPVC material has low strength and a rough surface that has limited its application.
[0162] The fluidity of polydimethylsiloxane KF-96H-30000CS is better than that of traditional silicones, and it is easier to disperse and wet the glass fiber. At the same time, the hyperbranched polar alkyl polyester can be used as a glass fiber compatibilizer and also as a flow modifier of polydimethylsiloxane KF-96H-30000CS, further improving its fluidity. The coordinated use of these components makes the glass fiber and CPVC resin fully compatible, thereby achieving good toughness, rigidity and a smooth surface.
[0163] The glass fiber reinforced CPVC material prepared by the stabilizer system of methyl tin mercaptan, pentaerythritol and glycerol has a dynamic stabilization time of more than 1400 seconds, which is 200 seconds longer than the traditional organic tin and hydrotalcite stabilization system, and is easier to process the CPVC material. Pentaerythritol can usually be used as an acid-absorbing stabilizer, but its melting point is about 250° C., and it will not melt at the material processing temperature. If it is not well dispersed, it will not achieve the expected stabilization effect. The glycerol introduced in the present invention can dissolve the pentaerythritol, and then disperse it evenly to play an unexpected stabilization effect, prolong the dynamic stabilization time of the CPVC material, and make it easier to process.
[0164] Depend on Figure 1-4 It can be seen that the surface of the sample of the embodiment of the present invention is smooth and has no floating fibers, while the surface of the sample of the comparative example is rough and has serious floating fibers. Further electron microscope observation shows that the glass fiber of the present invention has good bonding with the CPVC resin, and the glass fiber is completely wrapped by the CPVC resin, while the bonding between the glass fiber of the comparative example and the CPVC resin is very poor, and most of the glass fiber and the resin are separated.
[0165] The above description is only a preferred embodiment of the present invention and does not constitute any other form of limitation to the present invention. Any modification or equivalent change made based on the technical essence of the present invention still falls within the scope of protection required by the present invention.
Claims
1. A high-strength and high-slip glass fiber reinforced CPVC material, characterized in that: The composition comprises the following components in parts by weight: 60-80 parts of CPVC resin; Glass fiber 20-40 parts; 5-15 parts of toughening agent; Compatibilizer 0.5-2 parts; 2-6 parts of slip agent; 2-4 parts of stabilizer; Antioxidant 0.1-0.5 parts; Lubricant 0.5-2 parts; 1-2 parts of processing aid; The glass fiber reinforced CPVC material has a tensile strength of 65-80 MPa and an Izod beam notched impact strength of 65-70 J / m.
2. The glass fiber reinforced CPVC material according to claim 1, characterized in that: The glass fiber reinforced CPVC material has a bending strength of 90-110 MPa, a bending modulus of 8500-11500 MPa, a Vicat softening temperature of 126-130° C. 50N / 50° C., and a friction coefficient of 0.10-0.
20.
3. The glass fiber reinforced CPVC material according to claim 1 or 2, characterized in that: The toughening agent includes at least one of chlorinated polyethylene, ketone vinyl ester, and impact-resistant acrylic copolymer.
4. The glass fiber reinforced CPVC material according to claim 3, characterized in that: The toughening agent is a compound of chlorinated polyethylene and impact-resistant acrylic copolymer, with a mass ratio of 1:1 to 3:
1.
5. The glass fiber reinforced CPVC material according to claim 1 or 2, characterized in that: The compatibilizer is a hyperbranched polar alkyl polyester; the hyperbranched polar alkyl polyester is obtained by modifying the terminal hydroxyl hyperbranched polyester by terminal alkylation with hexadecanoyl chloride, the molecular weight of the terminal hydroxyl hyperbranched polyester is 6000-9000, the number of hydroxyl groups is 20-30 / mol, and the hydroxyl value is 100-200.
6. The glass fiber reinforced CPVC material according to claim 1 or 2, characterized in that: The slip agent is polydimethylsiloxane, with a viscosity of ≥30000mm at 25°C 2 / s.
7. The glass fiber reinforced CPVC material according to claim 1 or 2, characterized in that: The stabilizer is a compound of methyltin mercaptan, pentaerythritol and glycerol, with a mass ratio of 1:0.1:0.
4.
8. A method for preparing the glass fiber reinforced CPVC material according to any one of claims 1 to 7, characterized in that: The following steps are involved: Step A) preparing a stabilizer: compounding a stabilizer in a liquid mixer at a temperature of 70-90° C.; Step B) Mixing: First, weigh the CPVC resin powder, lubricant, antioxidant, stabilizer, compatibilizer, slip agent, toughening agent and processing aid in parts by weight and put them into a high mixing pot to mix into a premix; Step C) extrusion molding: the premix of step B) is added into the twin-screw extruder from the main feed port, the glass fiber is added into the twin-screw extruder from the side feed port, and melt extrusion, drawing and granulation are performed at a temperature of 160-180° C. to obtain the glass fiber reinforced CPVC material.
9. The preparation method according to claim 8, characterized in that: In step A), propylene glycol is first added into a liquid mixer, stirred at a low speed and heated to 80° C., then pentaerythritol is added, the temperature is stopped and stirred continuously until the pentaerythritol is completely dissolved, and then methyl tin mercaptan is added, and stirring is continued for 2 minutes until the mixture is evenly stirred to obtain the stabilizer.
10. The preparation method according to claim 9, characterized in that: In step B), first, CPVC resin powder, lubricant and antioxidant are added to a high mixing pot and mixed at a stirring rate of 100-200 rpm for 1-5 minutes, then a stabilizer is added and mixed at a stirring rate of 300-400 rpm for 1-5 minutes, then a compatibilizer and a slip agent are added and mixed for 1-5 minutes, and finally a toughening agent and a processing aid are added and mixed for 1-5 minutes. When all materials are mixed evenly, mixing is stopped and the premix is discharged into a storage tank for standby use.