Viscosity regulation and control method of shear thickening fluid and application of shear thickening fluid in composite structure

By using modified polymethyl methacrylate microspheres and nanosilicon dioxide in the shear thickening liquid, combined with polycarboxylate as a viscosity regulator, the problem of excessive tension between the dispersion medium and the dispersed phase is solved. , the stability and uniformity of the shear thickening liquid are improved, and the stability at high temperature and viscosity change characteristics are achieved at high shear rate.

CN118909377APending Publication Date: 2024-11-08范吉堂 +1
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410946118.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-15
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

In the viscosity control method of shear thickening liquid, the interface tension between the dispersed medium and the dispersed phase leads to particles aggregation, affecting the shear thickening performance and stability, and the dispersed medium is prone to instability at high temperatures.

Method used

Dispersion media is prepared by using materials such as glycerol, sodium silicate, polyethylene glycol and triethanolamine, and modified polymethyl methacrylate microspheres and nanosilicon dioxide, combined with polycarboxylate as viscosity regulators. Regulate the viscosity of the shear thickening liquid, form a stable interface layer to prevent particles from aggregation, and improve the stability and uniformity of the fluid.

Benefits of technology

Effectively reduces interfacial tension, enhances the adhesion between particles and dispersion medium, improves the stability and uniformity of the shear thickening liquid, maintains the stability at high temperature and the viscosity changes at high shear rates. characteristic.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004945678980000101
    Figure BDA0004945678980000101
  • Figure BDA0004945678980000111
    Figure BDA0004945678980000111
  • Figure BDA0004945678980000112
    Figure BDA0004945678980000112
Patent Text Reader

Abstract

The invention discloses a viscosity regulation and control method of a shear thickening fluid and application of the shear thickening fluid in a composite structure. The shear thickening fluid is prepared by mixing a dispersion phase and a dispersion medium according to a certain mass ratio and regulating and controlling by using a viscosity regulation and control agent, the modified methyl methacrylate microspheres are used as a dispersion phase to enhance the interaction between particles and a dispersion medium and reduce the interfacial tension, and the silanol compound can enhance the adhesion among the modified methyl methacrylate microspheres, the nano silicon dioxide and the dispersion medium. The interface tension among the methyl methacrylate microspheres, the nano silicon dioxide and the dispersion medium is reduced, and triethanolamine has relatively high thermal stability, can be used as a stable component of the dispersion medium in high-temperature application, and can maintain the uniformity and stability of the shear thickening fluid; the high-strength impact-resistant composite material has a wide application prospect in the fields of automobile bumpers, sports protection equipment, packaging materials, aerospace industry and other fields requiring high strength and impact resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of protective materials, in particular to a method for regulating the viscosity of a shear thickening fluid and an application thereof in a composite structure. Background Art

[0002] The field of protective materials is a discipline focused on the research, development and application of materials that can protect people, equipment or structures from physical, chemical or biological harm. These materials are designed to provide protection in a variety of environments, from everyday personal protective equipment to industrial and military applications. Shear-thickening fluid composites represent a major innovation in the field of protective materials. They combine the strength of traditional protective materials with the flexibility and intelligent response characteristics of modern composites. Shear-thickening fluid materials exhibit low viscosity under low shear stress, so they remain soft and comfortable under normal conditions, similar to liquids or semi-solid substances. However, when subjected to high speed or high shear force, their viscosity increases rapidly and becomes extremely hard, providing immediate protection.

[0003] Shear thickening fluid is prepared by a certain mass ratio of dispersed phase and dispersion medium. If the interfacial tension between the dispersion medium and the dispersed phase (solid particles) is too high, it will hinder the effective wetting and dispersion of the particles, which will cause the particles to aggregate instead of being evenly distributed, thus affecting the shear thickening performance and stability of STF. Most shear thickening fluids use water or organic solvents as dispersion media, which may evaporate or decompose at high temperatures, causing the system to become unstable, resulting in weak binding force between the dispersion medium and the dispersed phase and easy stratification of the system.

[0004] To this end, we propose a method for regulating the viscosity of shear thickening fluids and its application in composite structures. Summary of the invention

[0005] The purpose of the present application is to provide a method for regulating the viscosity of a shear thickening fluid and its application in a composite structure, which can effectively solve the problems raised in the above-mentioned background technology.

[0006] To achieve the above object, the technical solution adopted by the present invention is: a method for regulating the viscosity of a shear thickening liquid, wherein the shear thickening liquid is prepared by mixing a dispersed phase and a dispersion medium in a certain mass ratio and regulating the mixture using a viscosity regulator, comprising the following steps:

[0007] S1. Preparation of a dispersion medium: Add a required amount of glycerol and sodium silicate to a reaction kettle, stir them evenly to obtain an aqueous phase A, add an alkaline regulator until the pH value of the aqueous phase A is 7 to 8, heat the aqueous phase A to 45° C. to 65° C., and keep it warm, add polyethylene glycol and triethanolamine to the reaction kettle to obtain an aqueous phase B, and stir at a temperature of 45° C. to 65° C. to obtain a dispersion medium, wherein the pH value of the dispersion medium is 7 to 8;

[0008] S2. Preparation of shear thickening fluid: heat the dispersion medium to 80° C. to 140° C., add modified polymethyl methacrylate microspheres, nano-silica, polymethacrylic acid, polyvinyl pyrrolidone, and 3-aminopropyl triethoxysilane to the dispersion medium under continuous stirring, continue mechanical stirring for 2 hours after the addition is completed, and then use a ball mill to disperse the mechanically stirred system at 100 r / min for 2 hours, finally evacuate the system for 1 hour to appropriately remove bubbles in the system, and let it stand to obtain a shear thickening fluid;

[0009] S3, preparing a viscosity control agent: weighing a required amount of polycarboxylate powder and placing it in a magnetic stirrer, adding deionized water, and turning on the magnetic stirrer for stirring at a stirring speed of 300-500 rpm for 10-30 minutes until the polycarboxylate is completely dissolved, and adding a diluted sodium hydroxide solution dropwise to control the pH value between 7 and 9 to obtain a viscosity control agent;

[0010] S4, cooling the obtained shear thickening fluid to room temperature and placing it in a magnetic stirrer, slowly pouring in a viscosity control agent, and turning on the magnetic stirrer for stirring at a stirring speed of 200-500 rpm for 10-20 minutes to ensure uniform distribution, thereby obtaining a shear thickening liquid;

[0011] The viscosity regulator accounts for 3-15% of the mass fraction of the shear thickening fluid.

[0012] The shear thickening fluid comprises, by weight: 4-8 parts of glycerol, 7-12 parts of sodium silicate, 3-9 parts of polyethylene glycol, 4-8 parts of triethanolamine, 12-20 parts of modified polymethyl methacrylate microspheres, 4-8 parts of nano silicon dioxide, 0.4-1.2 parts of polymethacrylic acid, 0.2-1 parts of polyvinyl pyrrolidone, and 1.4-2.2 parts of 3-aminopropyl triethoxysilane;

[0013] Preferably, the viscosity regulator comprises, by weight: 6-12 parts of polycarboxylate and 12-18 parts of deionized water.

[0014] Preferably, the preparation method of the modified polymethyl methacrylate microspheres comprises the following steps:

[0015] S1. Pretreatment of polymethyl methacrylate microspheres: polymethyl methacrylate microspheres are selected, dispersed in isopropanol, subjected to ultrasonic treatment for a certain period of time to remove surface impurities, then centrifuged, the precipitate is collected, washed with isopropanol for multiple times, and finally dried;

[0016] S2. Preparation of graphite phase carbon nitride suspension: adding graphite phase carbon nitride to isopropanol, adding a stabilizer and a binder, and performing ultrasonic treatment until the graphite phase carbon nitride is completely dispersed to form a uniform suspension;

[0017] S3. Preparation of graphene oxide dispersion: adding graphene oxide powder to deionized water, and ultrasonically treating until the powder is completely dispersed to obtain a graphene oxide dispersion;

[0018] S4. Immerse the pretreated polymethyl methacrylate microspheres in a graphite phase carbon nitride suspension, perform ultrasonic treatment, centrifuge, wash, remove excess suspension, immerse the microspheres in a graphene oxide dispersion again, repeat the ultrasonic treatment, centrifuge and wash processes, repeat the above operations until 4-12 nanocomposite layers are formed on the surface of the polymethyl methacrylate microspheres, and obtain modified polymethyl methacrylate microspheres after drying and grinding.

[0019] Preferably, the modified polymethyl methacrylate microspheres include, by weight: 12-20 parts of polymethyl methacrylate microspheres, 12-22 parts of isopropyl alcohol, 2-8 parts of graphite phase carbon nitride, 1-4 parts of stabilizer, 2-6 parts of binder, 5-12 parts of graphene oxide powder, and 8-16 parts of deionized water.

[0020] Preferably, the stabilizer is acetic acid.

[0021] Preferably, the binder is chitosan.

[0022] Preferably, the particle size of the polymethyl methacrylate microspheres is 50 nm to 500 nm.

[0023] Preferably, in S4, a high-speed centrifuge is used for centrifugation at a speed of 200 rpm / s-500 rpm / s for 10 min.

[0024] The second aspect of the present invention provides an application of a shear thickening fluid. The prepared shear thickening fluid can be used in automobile bumpers, sports protective equipment, packaging materials, aerospace industry and other fields requiring high strength and impact resistance after being solidified.

[0025] Compared with the prior art, the present invention provides a method for regulating the viscosity of a shear thickening fluid and its application in a composite structure, which has the following beneficial effects:

[0026] 1. The triethanolamine in triethanolamine reacts with the silicate ions of sodium silicate to generate silanol compounds. The silanol compounds have certain surface activity and can be adsorbed on the surface of solid particles. The silanol compounds can enhance the adhesion between modified methyl methacrylate microspheres, nano-silica and the dispersion medium, and reduce the interfacial tension between methyl methacrylate microspheres, nano-silica and the dispersion medium. By forming a stable interface layer, the aggregation and sedimentation of solid particles are prevented. In addition, triethanolamine has high thermal stability and is not easy to volatilize. It can be used as a stable component of the dispersion medium in high-temperature applications and can maintain the uniformity and stability of the shear thickening fluid.

[0027] 2. Changing the surface properties of methyl methacrylate microspheres. In the process of preparing modified polymethyl methacrylate microspheres, graphite phase carbon nitride and graphene oxide were used to modify the surface of the microspheres, which improved the dispersibility of the particles, enhanced the interaction between the particles and the dispersion medium, and reduced the interfacial tension.

[0028] 3. The molecular structure of the polycarboxylate in the prepared viscosity regulator contains multiple carboxyl groups (-COOH), which can dissociate into negatively charged carboxylate ions (-COO-) in water, thereby forming negatively charged polymer chains in the solution. When the viscosity regulator is added to the shear thickening fluid, the negatively charged polymer chains can be adsorbed on the surface of dispersed phase particles such as modified polymethyl methacrylate microspheres and nano-silica. Since charges of the same kind repel each other, this electrostatic repulsion can prevent direct contact and aggregation between particles, maintain the uniform dispersion of particles in the fluid, and thus improve the stability and uniformity of the fluid. At low shear rates, these polymer chains can freely entangle together to form a three-dimensional network structure, thereby increasing the viscosity of the fluid. At high shear rates, the polymer chains are straightened, the network structure is destroyed, and the viscosity of the fluid decreases rapidly, showing shear thickening characteristics. DETAILED DESCRIPTION

[0029] In order to make the technical means, creative features, objectives and effects of the present invention easy to understand, the present invention will be further described below. Obviously, the embodiments described are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0030] In order to address the deficiencies of the prior art, the present invention provides a viscosity control method for a shear thickening fluid and an application thereof in a composite structure. The shear thickening fluid is prepared by mixing a dispersed phase and a dispersed medium in a certain mass ratio and regulating the mixture using a viscosity control agent, and the method comprises the following steps:

[0031] S1. Preparation of dispersion medium: Add the required amount of glycerol and sodium silicate to a reaction kettle, stir them evenly to obtain aqueous phase A, add an alkaline regulator until the pH value of aqueous phase A is 7-8, heat aqueous phase A to 45°C-65°C, and keep it warm, add polyethylene glycol and triethanolamine to the reaction kettle to obtain aqueous phase B, and stir at a temperature of 45°C-65°C to obtain a dispersion medium, wherein the pH value of the dispersion medium is 7-8;

[0032] S2. Preparation of shear thickening fluid: heat the dispersion medium to 80° C. to 140° C., add modified polymethyl methacrylate microspheres, nano-silica, polymethacrylic acid, polyvinyl pyrrolidone, and 3-aminopropyl triethoxysilane to the dispersion medium under continuous stirring, continue mechanical stirring for 2 hours after the addition is completed, and then use a ball mill to disperse the mechanically stirred system at 100 r / min for 2 hours, finally evacuate the system for 1 hour to appropriately remove bubbles in the system, and let it stand to obtain a shear thickening fluid;

[0033] S3, preparing a viscosity control agent: weighing a required amount of polycarboxylate powder and placing it in a magnetic stirrer, adding deionized water, and turning on the magnetic stirrer for stirring at a stirring speed of 300-500 rpm for 10-30 minutes until the polycarboxylate is completely dissolved, and adding a diluted sodium hydroxide solution dropwise to control the pH value between 7 and 9 to obtain a viscosity control agent;

[0034] S4, cooling the obtained shear thickening fluid to room temperature and placing it in a magnetic stirrer, slowly pouring in the viscosity control agent, and turning on the magnetic stirrer for stirring at a stirring speed of 200-500 rpm for 10-20 minutes to ensure uniform distribution, thereby obtaining a shear thickening liquid;

[0035] The viscosity regulator accounts for 9% of the shear thickening fluid by mass;

[0036] It should be noted that triethanolamine (TEA) and sodium silicate (Na2SiO3) can react to generate silanol compounds, and the reaction equation is as follows:

[0037] Na2SiO3+3TEA→Si(OH)3(CH2CH2NH)3+2Na+Na2SiO3+3TEA→Si(OH)3(CH2C

[0038] H2NH)3+2Na +

[0039] Silanol compounds (Si(OH)n) are adsorbed on the surface of solid particles, enhancing the adhesion between particles and the dispersion medium, reducing interfacial tension, and preventing particle aggregation and sedimentation;

[0040] As a viscosity regulator, polycarboxylates have multiple carboxyl groups (-COOH) in their molecular structure, which dissociate into negatively charged carboxylate ions (-COO-) in water. When added to shear thickening fluids, the negatively charged polymer chains adsorb on the surface of particles such as modified PMMA microspheres and nano-silica, preventing particle aggregation through electrostatic repulsion;

[0041] The shear thickening fluid comprises, by weight: 4-8 parts of glycerol, 7-12 parts of sodium silicate, 3-9 parts of polyethylene glycol, 4-8 parts of triethanolamine, 12-20 parts of modified polymethyl methacrylate microspheres, 4-8 parts of nano-silicon dioxide, 0.4-1.2 parts of polymethacrylic acid, 0.2-1 parts of polyvinyl pyrrolidone, and 1.4-2.2 parts of 3-aminopropyl triethoxysilane;

[0042] The viscosity control agent comprises, by weight: 6-12 parts of polycarboxylate and 12-18 parts of deionized water.

[0043] The preparation method of modified polymethyl methacrylate microspheres comprises the following steps:

[0044] S1. Pretreatment of polymethyl methacrylate microspheres: polymethyl methacrylate microspheres with a particle size of 50 nm to 500 nm are selected, dispersed in isopropanol, subjected to ultrasonic treatment for a certain period of time to remove surface impurities, then centrifuged, the precipitate is collected, washed with isopropanol for multiple times, and finally dried;

[0045] S2. Preparation of graphite phase carbon nitride suspension: adding graphite phase carbon nitride to isopropanol, adding a stabilizer and a binder, and performing ultrasonic treatment until the graphite phase carbon nitride is completely dispersed to form a uniform suspension;

[0046] S3. Preparation of graphene oxide dispersion: adding graphene oxide powder to deionized water, and ultrasonically treating until the powder is completely dispersed to obtain a graphene oxide dispersion;

[0047] S4, immersing the pretreated polymethyl methacrylate microspheres in a graphite phase carbon nitride suspension, ultrasonically treating, centrifuging, washing, removing excess suspension, immersing the microspheres in a graphene oxide dispersion again, repeating the ultrasonic treatment, centrifuging using a high-speed centrifuge at a speed of 200 rpm / s-500 rpm / s for 10 min, repeating the above operation, washing after centrifugation until 4-12 nanocomposite layers are formed on the surface of the polymethyl methacrylate microspheres, and obtaining modified polymethyl methacrylate microspheres after drying and grinding;

[0048] It should be noted that the surface modification of polymethyl methacrylate (PMMA) microspheres using graphite phase carbon nitride (g-C3N4) and graphene oxide (GO) improves the dispersibility of the particles and the interaction with the dispersion medium, further reducing the interfacial tension;

[0049] The modified polymethyl methacrylate microspheres include, by weight: 12-20 parts of polymethyl methacrylate microspheres, 12-22 parts of isopropyl alcohol, 2-8 parts of graphite phase carbon nitride, 1-4 parts of a stabilizer, 2-6 parts of a binder, 5-12 parts of graphene oxide powder, and 8-16 parts of deionized water;

[0050] The stabilizer is acetic acid;

[0051] The binder is chitosan.

[0052] Embodiment 1

[0053] The viscosity control method of the shear thickening liquid is as follows: the shear thickening liquid is prepared by mixing a dispersed phase and a dispersed medium in a certain mass ratio and controlling the mixture using a viscosity control agent, comprising the following steps:

[0054] S1. Preparation of dispersion medium: Add required amounts of glycerol and sodium silicate to a reaction kettle, stir them evenly to obtain aqueous phase A, add alkaline regulator until the pH value of aqueous phase A is 7-8, heat aqueous phase A to 55° C. and keep warm, add polyethylene glycol and triethanolamine to the reaction kettle to obtain aqueous phase B, stir at 55° C. to obtain dispersion medium, wherein the pH value of the dispersion medium is 7-8;

[0055] S2. Preparation of shear thickening fluid: heat the dispersion medium to 110° C., add modified polymethyl methacrylate microspheres, nano-silica, polymethacrylic acid, polyvinyl pyrrolidone, and 3-aminopropyl triethoxysilane to the dispersion medium under continuous stirring, continue mechanical stirring for 2 h after the addition is complete, and then use a ball mill to disperse the mechanically stirred system at 100 r / min for 2 h, finally evacuate the system for 1 h to properly remove bubbles in the system, and let it stand to obtain a shear thickening fluid;

[0056] S3, preparing a viscosity control agent: weighing a required amount of polycarboxylate powder and placing it in a magnetic stirrer, adding deionized water, and turning on the magnetic stirrer for stirring at a stirring speed of 400 rpm for 20 minutes until the polycarboxylate is completely dissolved, and adding a diluted sodium hydroxide solution dropwise to control the pH value between 7 and 9 to obtain a viscosity control agent;

[0057] S4, cooling the obtained shear thickening fluid to room temperature and placing it in a magnetic stirrer, slowly pouring in the viscosity control agent, and turning on the magnetic stirrer for stirring at a stirring speed of 200-500 rpm for 10-20 minutes to ensure uniform distribution, thereby obtaining a shear thickening liquid;

[0058] The viscosity regulator accounts for 9% of the shear thickening fluid by mass;

[0059] The shear thickening fluid comprises, by weight: 6 parts of glycerol, 10 parts of sodium silicate, 6 parts of polyethylene glycol, 6 parts of triethanolamine, 16 parts of modified polymethyl methacrylate microspheres, 6 parts of nano-silicon dioxide, 0.8 parts of polymethacrylic acid, 0.6 parts of polyvinyl pyrrolidone, and 1.8 parts of 3-aminopropyl triethoxysilane;

[0060] The viscosity control agent comprises, by weight: 9 parts of polycarboxylate and 15 parts of deionized water.

[0061] The preparation method of modified polymethyl methacrylate microspheres comprises the following steps:

[0062] S1. Pretreatment of polymethyl methacrylate microspheres: polymethyl methacrylate microspheres with a particle size of 50 nm to 500 nm are selected, dispersed in isopropanol, subjected to ultrasonic treatment for a certain period of time to remove surface impurities, then centrifuged, the precipitate is collected, washed with isopropanol for multiple times, and finally dried;

[0063] S2. Preparation of graphite phase carbon nitride suspension: adding graphite phase carbon nitride to isopropanol, adding a stabilizer and a binder, and performing ultrasonic treatment until the graphite phase carbon nitride is completely dispersed to form a uniform suspension;

[0064] S3. Preparation of graphene oxide dispersion: adding graphene oxide powder to deionized water, and ultrasonically treating until the powder is completely dispersed to obtain a graphene oxide dispersion;

[0065] S4, immersing the pretreated polymethyl methacrylate microspheres in a graphite phase carbon nitride suspension, ultrasonically treating, centrifuging, washing, removing excess suspension, immersing the microspheres in a graphene oxide dispersion again, repeating the ultrasonic treatment, centrifuging using a high-speed centrifuge at a speed of 300 rpm / s for 10 min, repeating the above operation, washing after centrifugation until 4-12 nanocomposite layers are formed on the surface of the polymethyl methacrylate microspheres, and obtaining modified polymethyl methacrylate microspheres after drying and grinding;

[0066] The modified polymethyl methacrylate microspheres include, by weight: 10 parts of polymethyl methacrylate microspheres, 12 parts of isopropyl alcohol, 5 parts of graphite phase nitridation, 2.5 parts of stabilizer, 4 parts of binder, 8 parts of graphene oxide powder, and 12 parts of deionized water;

[0067] The stabilizer is acetic acid;

[0068] The binder is chitosan.

[0069] Embodiment 2

[0070] The same preparation method as in Example 1 was followed, except that:

[0071] The shear thickening fluid comprises, by weight: 4 parts of glycerol, 7 parts of sodium silicate, 3 parts of polyethylene glycol, 4 parts of triethanolamine, 12 parts of modified polymethyl methacrylate microspheres, 4 parts of nano-silicon dioxide, 0.4 parts of polymethacrylic acid, 0.2 parts of polyvinyl pyrrolidone, and 1.4 parts of 3-aminopropyl triethoxysilane;

[0072] The viscosity control agent comprises, by weight: 9 parts of polycarboxylate and 15 parts of deionized water.

[0073] Embodiment 3

[0074] The same preparation method as in Example 1 was followed, except that:

[0075] The shear thickening fluid comprises, by weight: 8 parts of glycerol, 12 parts of sodium silicate, 9 parts of polyethylene glycol, 8 parts of triethanolamine, 20 parts of modified polymethyl methacrylate microspheres, 8 parts of nano-silicon dioxide, 1.2 parts of polymethacrylic acid, 1 part of polyvinyl pyrrolidone, and 2.2 parts of 3-aminopropyl triethoxysilane;

[0076] The viscosity control agent comprises, by weight: 9 parts of polycarboxylate and 15 parts of deionized water.

[0077] Comparative Example 1

[0078] The difference from the first embodiment is that:

[0079] The shear thickening fluid is prepared by mixing a dispersed phase and a dispersed medium in a certain mass ratio and regulating the mixture using a viscosity regulator, comprising the following steps:

[0080] S1. Preparation of dispersion medium: Add required amounts of glycerol and sodium silicate to a reaction kettle, stir them evenly to obtain aqueous phase A, add alkaline regulator until the pH value of aqueous phase A is 7-8, heat aqueous phase A to 55° C. and keep warm, add polyethylene glycol and triethanolamine to the reaction kettle to obtain aqueous phase B, stir at 55° C. to obtain dispersion medium, wherein the pH value of the dispersion medium is 7-8;

[0081] S2. Preparation of shear thickening fluid: heat the dispersion medium to 110° C., add nano-silicon dioxide, polymethacrylic acid, polyvinyl pyrrolidone and 3-aminopropyltriethoxysilane to the dispersion medium under continuous stirring, continue mechanical stirring for 2 h after the addition is completed, and then use a ball mill to disperse the mechanically stirred system at 100 r / min for 2 h, finally evacuate the system for 1 h to properly remove bubbles in the system, and let it stand to obtain a shear thickening fluid;

[0082] S3, preparing a viscosity control agent: weighing a required amount of polycarboxylate powder and placing it in a magnetic stirrer, adding deionized water, and turning on the magnetic stirrer for stirring at a stirring speed of 400 rpm for 20 minutes until the polycarboxylate is completely dissolved, and adding a diluted sodium hydroxide solution dropwise to control the pH value between 7 and 9 to obtain a viscosity control agent;

[0083] S4, cooling the obtained shear thickening fluid to room temperature and placing it in a magnetic stirrer, slowly pouring in the viscosity control agent, and turning on the magnetic stirrer for stirring at a stirring speed of 200-500 rpm for 10-20 minutes to ensure uniform distribution, thereby obtaining a shear thickening liquid;

[0084] The viscosity regulator accounts for 9% of the shear thickening fluid by mass;

[0085] The shear thickening fluid comprises, by weight: 6 parts of glycerol, 10 parts of sodium silicate, 6 parts of polyethylene glycol, 6 parts of triethanolamine, 24 parts of nano-silicon dioxide, 0.8 parts of polymethacrylic acid, 0.6 parts of polyvinyl pyrrolidone, and 1.8 parts of 3-aminopropyltriethoxysilane;

[0086] The viscosity control agent comprises, by weight: 9 parts of polycarboxylate and 15 parts of deionized water.

[0087] Comparative Example 2

[0088] The difference from the first embodiment is that:

[0089] The shear thickening fluid is prepared by mixing a dispersed phase and a dispersed medium in a certain mass ratio and regulating the mixture using a viscosity regulator, comprising the following steps:

[0090] S1. Preparation of dispersion medium: Add required amounts of glycerol and sodium silicate to a reaction kettle, stir them evenly to obtain aqueous phase A, add alkaline regulator until the pH value of aqueous phase A is 7-8, heat aqueous phase A to 55° C. and keep warm, add polyethylene glycol and triethanolamine to the reaction kettle to obtain aqueous phase B, stir at 55° C. to obtain dispersion medium, wherein the pH value of the dispersion medium is 7-8;

[0091] S2. Preparation of shear thickening fluid: heat the dispersion medium to 110° C., add modified polymethyl methacrylate microspheres, nano-silica, polymethacrylic acid, polyvinyl pyrrolidone, and 3-aminopropyl triethoxysilane to the dispersion medium under continuous stirring, continue mechanical stirring for 2 h after the addition is complete, and then use a ball mill to disperse the mechanically stirred system at 100 r / min for 2 h, finally evacuate the system for 1 h to properly remove bubbles in the system, and let it stand to obtain a shear thickening fluid;

[0092] S4, cooling the obtained shear thickening fluid to room temperature and placing it in a magnetic stirrer, turning on the magnetic stirrer for stirring, setting the stirring speed at 200-500 rpm, stirring for 10-20 minutes to ensure uniform distribution, and obtaining a shear thickening liquid;

[0093] The shear thickening fluid comprises, by weight: 6 parts of glycerol, 10 parts of sodium silicate, 6 parts of polyethylene glycol, 6 parts of triethanolamine, 16 parts of modified polymethyl methacrylate microspheres, 6 parts of nano-silicon dioxide, 0.8 parts of polymethacrylic acid, 0.6 parts of polyvinyl pyrrolidone, and 1.8 parts of 3-aminopropyltriethoxysilane.

[0094] Comparative Example 3

[0095] The difference from the first embodiment is that:

[0096] The shear thickening fluid is prepared by mixing a dispersed phase and a dispersed medium in a certain mass ratio and regulating the mixture using a viscosity regulator, comprising the following steps:

[0097] S1. Preparation of dispersion medium: Add required amounts of glycerol and sodium silicate to a reaction kettle, stir them evenly to obtain aqueous phase A, add an alkaline regulator until the pH value of aqueous phase A is 7-8, heat aqueous phase A to 55° C. and keep it warm, add polyethylene glycol to the reaction kettle to obtain aqueous phase B, stir them at 55° C. to obtain a dispersion medium, and the pH value of the dispersion medium is 7-8;

[0098] S2. Preparation of shear thickening fluid: heat the dispersion medium to 110° C., add modified polymethyl methacrylate microspheres, nano-silica, polymethacrylic acid, polyvinyl pyrrolidone, and 3-aminopropyl triethoxysilane to the dispersion medium under continuous stirring, continue mechanical stirring for 2 h after the addition is complete, and then use a ball mill to disperse the mechanically stirred system at 100 r / min for 2 h, finally evacuate the system for 1 h to properly remove bubbles in the system, and let it stand to obtain a shear thickening fluid;

[0099] S3, preparing a viscosity control agent: weighing a required amount of polycarboxylate powder and placing it in a magnetic stirrer, adding deionized water, and turning on the magnetic stirrer for stirring at a stirring speed of 400 rpm for 20 minutes until the polycarboxylate is completely dissolved, and adding a diluted sodium hydroxide solution dropwise to control the pH value between 7 and 9 to obtain a viscosity control agent;

[0100] S4, cooling the obtained shear thickening fluid to room temperature and placing it in a magnetic stirrer, slowly pouring in the viscosity control agent, and turning on the magnetic stirrer for stirring at a stirring speed of 200-500 rpm for 10-20 minutes to ensure uniform distribution, thereby obtaining a shear thickening liquid;

[0101] The viscosity regulator accounts for 9% of the shear thickening fluid by mass;

[0102] The shear thickening fluid comprises, by weight: 6 parts of glycerol, 10 parts of sodium silicate, 6 parts of polyethylene glycol, 16 parts of modified polymethyl methacrylate microspheres, 6 parts of nano-silicon dioxide, 0.8 parts of polymethacrylic acid, 0.6 parts of polyvinyl pyrrolidone, and 1.8 parts of 3-aminopropyl triethoxysilane;

[0103] The viscosity control agent comprises, by weight: 9 parts of polycarboxylate and 15 parts of deionized water.

[0104] The shear thickening liquid prepared in Examples 1-3 and Comparative Examples 1-3 was taken, and the shear thickening liquid was preheated to 80° C. to improve its fluidity and processability. The preheated shear thickening liquid was fed into the hopper of the injection molding machine, and pushed into the heating cylinder by the screw. The shear thickening liquid was injected into the aluminum alloy mold under high pressure to ensure that the material evenly filled the entire mold space, and vulcanized at 100° C. and 20 MPa for 15 minutes to obtain a shear thickening composite material and test its performance through the following tests;

[0105] The shear thickening composite material samples prepared in Examples 1-3 and Comparative Examples 1-3 were subjected to ball rebound test (GB / T6670-1997) and high and low temperature impact test (EN 1621-1:2012). The specific test results are shown in Table 1:

[0106]

[0107]

[0108] Table 1

[0109] The test results in Table 1 show that the rebound percentages of Examples 1 to 3 are between 4.6% and 4.8%, and the rebound percentages of Comparative Examples 1 to 3 are between 4.1% and 4.2%. The Examples and Comparative Examples perform similarly in this test, and the difference in rebound rate is not large.

[0110] The impact attenuation force of Examples 1 to 3 is between 17.3-18.5 KN, and the impact attenuation force of Comparative Examples 1 to 3 is between 15.3-16.2 KN. It can be concluded that the impact attenuation performance of Examples 1 to 3 is better than that of the Comparative Examples. It can be seen that the shear thickening composite material in the embodiments has a higher impact attenuation performance. After high-temperature aging at 70°C, the impact attenuation force of Examples 1 to 3 is between 16.5-17.7 KN, and the impact attenuation force of Comparative Examples 1 to 3 is between 9.3-13.2 KN. It can be seen that the shear thickening composite material in the embodiments still maintains a higher impact attenuation performance. It can be obtained that the introduction of viscosity regulator, modified polymethyl methacrylate microspheres and triethanolamine improves the stability of the shear thickening material to a certain extent.

[0111] The shear thickening composite material samples prepared in Examples 1-3 and Comparative Examples 1-3 were subjected to a 10J kinetic energy impact test. The specific test results are shown in Table 2:

[0112]

[0113] Table 2

[0114] The test results in Table 2 show that the shear thickening composite materials prepared in Examples 1 to 3 show a lower depression ratio (6.4%, 7.9%, 7.3%) after being subjected to a 10J kinetic energy impact, which indicates that these materials have high toughness, can effectively absorb and disperse impact energy, and reduce deformation. The depression ratios of Comparative Examples 1 to 3 are 10.2%, 11.7% and 13.1%, respectively, which are significantly higher than those of the embodiment group, and the degree of damage to the appearance of the material after the impact is also more serious. It can be concluded that the introduction of modified polymethyl methacrylate microspheres and triethanolamine plays a key role in enhancing the toughness and impact resistance of the material, so that the material can better absorb and disperse the impact energy, thereby reducing deformation and damage when subjected to impact, and as an impact-resistant material, it has strong thermal stability and can maintain its performance over a wide temperature range. It has broad application prospects in automobile bumpers, sports protective equipment, packaging materials, aerospace industry and other fields requiring high strength and impact resistance.

[0115] The basic principles and main features of the present invention and the advantages of the present invention are shown and described above. Those skilled in the art should understand that the present invention is not limited to the above embodiments. The above embodiments and descriptions are only for illustrating the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, and these changes and improvements all fall within the scope of the present invention to be protected.

Claims

1. A method for regulating the viscosity of a shear thickening fluid, characterized in that: The shear thickening fluid is prepared by mixing a dispersed phase and a dispersed medium in a certain mass ratio and regulating the mixture using a viscosity regulator, comprising the following steps: S1. Preparation of a dispersion medium: Add a required amount of glycerol and sodium silicate to a reaction kettle, stir them evenly to obtain an aqueous phase A, add an alkaline regulator until the pH value of the aqueous phase A is 7 to 8, heat the aqueous phase A to 45° C. to 65° C., and keep it warm, add polyethylene glycol and triethanolamine to the reaction kettle to obtain an aqueous phase B, and stir at a temperature of 45° C. to 65° C. to obtain a dispersion medium, wherein the pH value of the dispersion medium is 7 to 8; S2. Preparation of shear thickening fluid: heat the dispersion medium to 80° C. to 140° C., add modified polymethyl methacrylate microspheres, nano-silica, polymethacrylic acid, polyvinyl pyrrolidone, and 3-aminopropyl triethoxysilane to the dispersion medium under continuous stirring, continue mechanical stirring for 2 hours after the addition is completed, and then use a ball mill to disperse the mechanically stirred system at 100 r / min for 2 hours, finally evacuate the system for 1 hour to appropriately remove bubbles in the system, and let it stand to obtain a shear thickening fluid; S3, preparing a viscosity control agent: weighing a required amount of polycarboxylate powder and placing it in a magnetic stirrer, adding deionized water, and turning on the magnetic stirrer for stirring at a stirring speed of 300-500 rpm for 10-30 minutes until the polycarboxylate is completely dissolved, and adding a diluted sodium hydroxide solution dropwise to control the pH value between 7 and 9 to obtain a viscosity control agent; S4, cooling the obtained shear thickening fluid to room temperature and placing it in a magnetic stirrer, slowly pouring in a viscosity control agent, and turning on the magnetic stirrer for stirring at a stirring speed of 200-500 rpm for 10-20 minutes to ensure uniform distribution, thereby obtaining a shear thickening liquid; The viscosity regulator accounts for 3-15% of the mass fraction of the shear thickening fluid; The shear thickening fluid comprises, by weight: 4-8 parts of glycerol, 7-12 parts of sodium silicate, 3-9 parts of polyethylene glycol, 4-8 parts of triethanolamine, 12-20 parts of modified polymethyl methacrylate microspheres, 4-8 parts of nano silicon dioxide, 0.4-1.2 parts of polymethacrylic acid, 0.2-1 parts of polyvinyl pyrrolidone, and 1.4-2.2 parts of 3-aminopropyltriethoxysilane.

2. The method for controlling the viscosity of a shear thickening fluid according to claim 1, wherein: The viscosity control agent comprises, by weight: 6-12 parts of polycarboxylate and 12-18 parts of deionized water.

3. The method for controlling the viscosity of a shear thickening fluid according to claim 2, wherein: The preparation method of the modified polymethyl methacrylate microspheres comprises the following steps: S1. Pretreatment of polymethyl methacrylate microspheres: polymethyl methacrylate microspheres are selected, dispersed in isopropanol, subjected to ultrasonic treatment for a certain period of time to remove surface impurities, then centrifuged, the precipitate is collected, washed with isopropanol for multiple times, and finally dried; S2. Preparation of graphite phase carbon nitride suspension: adding graphite phase carbon nitride to isopropanol, adding a stabilizer and a binder, and performing ultrasonic treatment until the graphite phase carbon nitride is completely dispersed to form a uniform suspension; S3. Preparation of graphene oxide dispersion: adding graphene oxide powder to deionized water, and ultrasonically treating until the powder is completely dispersed to obtain a graphene oxide dispersion; S4. Immerse the pretreated polymethyl methacrylate microspheres in a graphite phase carbon nitride suspension, perform ultrasonic treatment, centrifuge, wash, remove excess suspension, immerse the microspheres in a graphene oxide dispersion again, repeat the ultrasonic treatment, centrifuge and wash processes, repeat the above operations until 4-12 nanocomposite layers are formed on the surface of the polymethyl methacrylate microspheres, and obtain modified polymethyl methacrylate microspheres after drying and grinding.

4. The method for controlling the viscosity of a shear thickening fluid according to claim 3, characterized in that: The modified polymethyl methacrylate microspheres include, by weight: 12-20 parts of polymethyl methacrylate microspheres, 12-22 parts of isopropyl alcohol, 2-8 parts of graphite phase carbon nitride, 1-4 parts of a stabilizer, 2-6 parts of a binder, 5-12 parts of graphene oxide powder, and 8-16 parts of deionized water.

5. The method for controlling the viscosity of a shear thickening fluid according to claim 4, characterized in that: The stabilizer is acetic acid.

6. The method for controlling the viscosity of a shear thickening fluid according to claim 4, characterized in that: The binder is chitosan.

7. The method for controlling the viscosity of a shear thickening fluid according to claim 3, characterized in that: The particle size of the polymethyl methacrylate microspheres is 50nm to 500nm.

8. The method for controlling the viscosity of a shear thickening fluid according to claim 3, characterized in that: In S4, a high-speed centrifuge is used for centrifugation at a speed of 200 rpm / s-500 rpm / s for 10 minutes.

9. Use of the shear thickening fluid obtained by the viscosity control method of the shear thickening fluid according to any one of claims 1 to 7, characterized in that: The resulting shear thickening fluid, after curing, can be used in automotive bumpers, sports protective equipment, packaging materials, the aerospace industry, and other fields requiring high strength and impact resistance.

Citation Information

Cited By

  • Impact-resistant flexible yarn with multi-spiral composite structure and preparation method of impact-resistant flexible yarn

    CN120575369A