Environment-friendly thermocuring impregnant and preparation method thereof

By combining and preparing environmentally friendly thermosetting impregnating agents, the defects of castings, weldments, and die-cast parts have been solved, achieving efficient and long-lasting repair results, improving the performance and lifespan of mechanical parts, and meeting environmental protection requirements.

CN118909382APending Publication Date: 2024-11-08BOTOU QIYUAN MASCH EQUIP MFG CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410976274.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-20
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Existing technologies have defects such as sand holes, pores and cracks in castings, welded parts and die-cast parts. Traditional repair methods are time-consuming and labor-intensive and difficult to completely solve the problem, and there is a lack of environmentally friendly and efficient repair materials.

Method used

An environmentally friendly thermosetting impregnating agent is used, which is composed of triethylene glycol dimethacrylate, vinyltris(trimethylsiloxane)silane, EDTA, polyvinyl alcohol, carbon black, initiator and polymerization inhibitor, etc. It forms a cross-linked network through ultrasonic mixing and high temperature reaction to achieve deep defect repair.

Benefits of technology

It achieves efficient and durable defect repair, improves the overall performance and lifespan of mechanical components, meets environmental protection requirements, and is applicable to various mechanical manufacturing fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118909382A_ABST
    Figure CN118909382A_ABST
Patent Text Reader

Abstract

The invention discloses an environment-friendly thermocuring impregnant and a preparation method thereof, and belongs to the technical field of nano materials. The preparation method comprises the following steps: ultrasonically mixing triethylene glycol dimethacrylate, vinyltris (trimethylsiloxane) silane, EDTA, polyvinyl alcohol, carbon black, an initiator, a polymerization inhibitor and a surfactant uniformly, transferring into a reaction kettle for high-temperature reaction, cooling, and storing at low temperature. The environment-friendly thermocuring impregnant has obvious advantages in efficiency, environmental protection and application range. The invention not only provides a new solution for solving common defects in mechanical manufacturing, but also contributes to promotion of green manufacturing and sustainable development of the industry.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of nano materials, and in particular relates to an environmentally friendly heat-curing impregnating agent and a preparation method thereof. Background Art

[0002] In the current mechanical manufacturing field, a series of defects such as sand holes, pores, cracks, and voids often occur during the production process of parts such as castings, weldments, and die-castings. These defects not only affect the appearance quality of the parts, but also seriously threaten their performance and life, bringing great difficulties and economic losses to maintenance and subsequent use. Traditional treatment methods mostly rely on subsequent repair work, such as welding, sand filling, compaction, etc., but these methods are often time-consuming and labor-intensive, and it is difficult to completely solve the problem, and sometimes even introduce new defects. Therefore, exploring a new, efficient material and method that can fundamentally solve the defect problem has become an urgent need in the industry.

[0003] In recent years, with the increasing requirements for environmental protection and the popularization of the concept of green manufacturing, the development of a new material that can efficiently repair defects and meet environmental protection requirements has become a research hotspot. In this context, an environmentally friendly thermosetting infiltrant and its preparation method introduced in this article are based on this demand. The environmentally friendly thermosetting infiltrant is mainly composed of a main material, a coagulating agent, a coupling agent, a cross-linking agent and a surfactant. Through the precise proportioning and optimization of these components, it can effectively penetrate into the sand holes, pores and cracks of parts such as castings, weldments and die-castings to achieve efficient and lasting repair, and ensure the environmental protection and safety of the entire process.

[0004] Compared with the prior art, the environmentally friendly thermosetting infiltrant of the present invention has the following significant advantages: first, through the optimized material combination and preparation method, deeper and more efficient defect repair can be achieved, greatly improving the overall performance and life of mechanical parts; second, the environmental performance of the infiltrant is significant, which not only meets the current high standards for environmental protection, but also ensures the health and safety of operators; finally, this material and method have a wide range of applications, not only suitable for the repair of traditional parts such as castings, weldments and die-castings, but can also be expanded to more mechanical manufacturing fields, and has a good market application prospect.

[0005] In particular, compared with other related products and technologies in this field, the environmentally friendly thermosetting impregnant of the present invention has obvious advantages in efficiency, environmental protection and application range. It not only provides a new solution to solve the common defect problems in mechanical manufacturing, but also contributes to promoting green manufacturing and sustainable development in the industry. Therefore, the development of this new impregnant undoubtedly has important theoretical value and practical application value. Summary of the invention

[0006] 1. Problems to be solved

[0007] In view of the above-mentioned deficiencies in the prior art, the purpose of the present invention is to provide an environmentally friendly thermosetting impregnant and a preparation method thereof, which has obvious advantages in efficiency, environmental friendliness and application range. It not only provides a new solution to solve the common defects in mechanical manufacturing, but also contributes to promoting green manufacturing and sustainable development in the industry.

[0008] 2. Technical solution

[0009] To solve the above problems, the technical solution provided by the present invention is:

[0010] An environmentally friendly heat-curing impregnating agent comprises the following raw materials in parts by weight:

[0011] Triethylene glycol dimethacrylate: 50-80 parts;

[0012] Vinyl tris(trimethylsiloxy)silane: 60-90 parts;

[0013] EDTA: 10-20 parts;

[0014] Polyvinyl alcohol: 10-25 parts;

[0015] Carbon black: 2-10 parts;

[0016] Initiator: 10-20 parts;

[0017] Inhibitor: 2-10 parts;

[0018] Surfactant: 5-15 parts.

[0019] The environmentally friendly heat-curing impregnating agent comprises the following raw materials in parts by weight:

[0020] Triethylene glycol dimethacrylate: 55-70 parts;

[0021] Vinyl tris(trimethylsiloxy)silane: 65-80 parts;

[0022] EDTA: 10-15 parts;

[0023] Polyvinyl alcohol: 10-20 parts;

[0024] Carbon black: 2-10 parts;

[0025] Initiator: 10-20 parts;

[0026] Inhibitor: 2-10 parts;

[0027] Surfactant: 5-15 parts.

[0028] The environmentally friendly heat-curing impregnating agent comprises the following raw materials in parts by weight:

[0029] Triethylene glycol dimethacrylate: 65 parts;

[0030] Vinyl tris(trimethylsiloxy)silane: 75 parts;

[0031] EDTA: 13 parts;

[0032] Polyvinyl alcohol: 15 parts;

[0033] Carbon black: 6 parts;

[0034] Initiator: 15 parts;

[0035] Inhibitor: 8 parts;

[0036] Surfactant: 10 parts.

[0037] The parameters of the environmentally friendly heat-curing impregnating agent and the triethylene glycol dimethacrylate are as follows: CAS No. 109-16-0, density 1.063 g / cm 3 ;

[0038] The parameters of the vinyl tris(trimethylsiloxy)silane are as follows: CAS No. 5356-84-3, density 0.861 g / mL.

[0039] The environmentally friendly heat-curing impregnating agent, the initiator is diisopropyl peroxydicarbonate or benzoyl peroxide;

[0040] The inhibitor is one of sodium pyrosulfite, tert-butylquinone, dibutylhydroxytoluene, and 2,6-dibutyl-p-cresol;

[0041] The surfactant is one of polysorbate, alkylphenol polyoxyethylene ether, tetraalkylammonium chloride, sodium lauryl sulfate and cocamidopropyl betaine.

[0042] The method for preparing the environmentally friendly heat-curing impregnating agent as described above comprises the following steps:

[0043] After ultrasonically mixing triethylene glycol dimethacrylate, vinyl tri(trimethylsiloxy)silane, EDTA, polyvinyl alcohol, carbon black, initiator, inhibitor and surfactant, the ultrasonic mixing temperature is 50°C-60°C, the ultrasonic mixing time is 2h-6h, the ultrasonic mixing power is 300W-600W, and then transferred to a reactor for high-temperature reaction, the high-temperature reaction temperature is 80°C-95°C, the high-temperature reaction time is 6h-12h, and after cooling, it is stored at low temperature.

[0044] The environmentally friendly heat-curing infiltrant formulation provided includes triethylene glycol dimethacrylate, vinyl tris(trimethylsiloxy)silane, EDTA and polyvinyl alcohol. Although the specific chemical reaction depends on experimental conditions such as temperature, pressure, the presence of catalysts, etc., several reaction mechanisms between these components can be obtained.

[0045] Cross-linking reaction:

[0046] The acrylate part of triethylene glycol dimethacrylate and the vinyl group of vinyl tris(trimethylsiloxy)silane can undergo free radical polymerization under appropriate conditions through a free radical initiator to form a cross-linked network. This is the main chemical reaction path for forming a thermal curing network, which is responsible for the curing of the impregnant and the formation of a stable structure.

[0047] Hydrolysis and condensation reactions:

[0048] Vinyl tris(trimethylsiloxy)silane undergoes hydrolysis reaction under high temperature or water conditions to form silanol groups. These silanol groups can further cross-link through condensation reaction to form a stable silicon-oxygen network structure, enhancing the thermal and chemical stability of the material.

[0049] Interaction with EDTA:

[0050] Although EDTA (ethylenediaminetetraacetic acid) is mainly used as a chelating agent to stabilize metal ions in the formulation to prevent metal-catalyzed premature polymerization or degradation reactions, in theory, the carboxyl groups it contains can also undergo esterification reactions with vinyl or acrylate groups. However, the occurrence of this reaction is low because it requires more specific conditions.

[0051] Interaction with polyvinyl alcohol:

[0052] Polyvinyl alcohol (PVA) is mainly introduced as a stabilizer, thickener or film former. Although PVA itself does not react chemically with the above monomers, it can physically affect the viscosity and film-forming properties of the impregnant system.

[0053] In summary, under typical preparation conditions, these components mainly form a stable cross-linked network through free radical polymerization and condensation reactions. The role of EDTA is mainly to prevent unexpected catalytic reactions by chelating metal ions, while polyvinyl alcohol mainly affects the properties of the system through physical means.

[0054] 3. Beneficial effects

[0055] The present invention discloses an environmentally friendly heat-curing impregnating agent and a preparation method thereof. The technology has the following significant advantages:

[0056] Efficient defect repair: Through optimized material combinations and preparation methods, deeper and more efficient defect repair can be achieved, greatly improving the overall performance and life of mechanical components.

[0057] Excellent environmental performance: The raw materials and preparation process of the impregnation agent meet environmental protection requirements, do not contain substances harmful to the environment, meet the current high standards for environmental protection, and also ensure the health and safety of operators.

[0058] Wide range of applications: It is not only suitable for the repair of traditional parts such as castings, weldments and die-castings, but can also be expanded to more mechanical manufacturing fields and has good market application prospects.

[0059] Compared with the prior art, the environmentally friendly thermosetting impregnant of the present invention has obvious advantages in efficiency, environmental friendliness and application range. It not only provides a new solution to solve the common defects in mechanical manufacturing, but also contributes to promoting green manufacturing and sustainable development in the industry.

[0060] Comparative test results

[0061] Comparative example tests show that the environmentally friendly heat-curing impregnating agent of the present invention has the following technical effects:

[0062] Replacing (meth)acrylate with triethylene glycol dimethacrylate can improve the high temperature resistance of the infiltrant.

[0063] Replacing triethylene glycol dimethacrylate with trimethylolpropane ester can improve the water resistance of the infiltrant.

[0064] Replacing vinyltris(trimethylsiloxy)silane with styryltrimethoxysilane can improve the corrosion resistance of the infiltrant.

[0065] Removing the PVA reduces the viscosity of the infiltrant, allowing it to penetrate defects more easily.

[0066] Eliminating EDTA can reduce the cost of the infiltrant. BRIEF DESCRIPTION OF THE DRAWINGS

[0067] Figure 1 This is a physical picture of the product prepared in Example 5 of the present invention. DETAILED DESCRIPTION

[0068] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0069] It should be noted that, in the present invention, all weight parts involved are kilograms (Kg).

[0070] It should be noted that, in the present invention, all reagents were purchased from Sinopharm Chemical Reagent Co., Ltd.

[0071] Example 1

[0072] The environmentally friendly heat-curing impregnating agent comprises the following raw materials in parts by weight:

[0073] Triethylene glycol dimethacrylate: 50 parts;

[0074] Vinyl tris(trimethylsiloxy)silane: 90 parts;

[0075] EDTA: 10 parts;

[0076] Polyvinyl alcohol: 25 parts;

[0077] Carbon black: 2 parts;

[0078] Initiator: 20 parts;

[0079] Inhibitor: 2 parts;

[0080] Surfactant: 15 parts.

[0081] The parameters of the environmentally friendly heat-curing impregnating agent and the triethylene glycol dimethacrylate are as follows: CAS No. 109-16-0, density 1.063 g / cm 3 ;

[0082] The parameters of the vinyl tris(trimethylsiloxy)silane are as follows: CAS No. 5356-84-3, density 0.861 g / mL.

[0083] The environmentally friendly heat-curing impregnating agent, the initiator is diisopropyl peroxydicarbonate;

[0084] The inhibitor is sodium pyrosulfite;

[0085] The surfactant is polysorbate.

[0086] The method for preparing the environmentally friendly heat-curing impregnating agent as described above comprises the following steps:

[0087] After ultrasonically mixing triethylene glycol dimethacrylate, vinyl tri(trimethylsiloxy)silane, EDTA, polyvinyl alcohol, carbon black, initiator, inhibitor and surfactant at a temperature of 50°C, a time of 6 hours and a power of 300W, the mixture is transferred to a reactor for high-temperature reaction at a temperature of 80°C and a time of 12 hours. After cooling, the mixture is stored at a low temperature.

[0088] Example 2

[0089] The environmentally friendly heat-curing impregnating agent comprises the following raw materials in parts by weight:

[0090] Triethylene glycol dimethacrylate: 80 parts;

[0091] Vinyl tris(trimethylsiloxy)silane: 60 parts;

[0092] EDTA: 20 parts;

[0093] Polyvinyl alcohol: 10 parts;

[0094] Carbon black: 10 parts;

[0095] Initiator: 10 parts;

[0096] Inhibitor: 10 parts;

[0097] Surfactant: 5 parts.

[0098] The parameters of the environmentally friendly heat-curing impregnating agent and the triethylene glycol dimethacrylate are as follows: CAS No. 109-16-0, density 1.063 g / cm 3 ;

[0099] The parameters of the vinyl tris(trimethylsiloxy)silane are as follows: CAS No. 5356-84-3, density 0.861 g / mL.

[0100] The environmentally friendly heat-curing impregnating agent, the initiator is benzoyl peroxide;

[0101] The polymerization inhibitor is tert-butylquinone;

[0102] The surfactant is tetraalkylammonium chloride.

[0103] The method for preparing the environmentally friendly heat-curing impregnating agent as described above comprises the following steps:

[0104] After ultrasonically mixing triethylene glycol dimethacrylate, vinyl tri(trimethylsiloxy)silane, EDTA, polyvinyl alcohol, carbon black, initiator, inhibitor and surfactant at a temperature of 60°C, a time of 2 hours and a power of 600W, the mixture is transferred to a reactor for high-temperature reaction at a temperature of 95°C and a time of 6 hours. After cooling, the mixture is stored at a low temperature.

[0105] Example 3

[0106] The environmentally friendly heat-curing impregnating agent comprises the following raw materials in parts by weight:

[0107] Triethylene glycol dimethacrylate: 55 parts;

[0108] Vinyl tris(trimethylsiloxy)silane: 80 parts;

[0109] EDTA: 10 parts;

[0110] Polyvinyl alcohol: 20 parts;

[0111] Carbon black: 2 parts;

[0112] Initiator: 20 parts;

[0113] Inhibitor: 2 parts;

[0114] Surfactant: 15 parts.

[0115] The parameters of the environmentally friendly heat-curing impregnating agent and the triethylene glycol dimethacrylate are as follows: CAS No. 109-16-0, density 1.063 g / cm 3 ;

[0116] The parameters of the vinyl tris(trimethylsiloxy)silane are as follows: CAS No. 5356-84-3, density 0.861 g / mL.

[0117] The environmentally friendly heat-curing impregnating agent, the initiator is diisopropyl peroxydicarbonate;

[0118] The inhibitor is butylated hydroxytoluene;

[0119] The surfactant is sodium lauryl sulfate.

[0120] The method for preparing the environmentally friendly heat-curing impregnating agent as described above comprises the following steps:

[0121] After ultrasonically mixing triethylene glycol dimethacrylate, vinyl tri(trimethylsiloxy)silane, EDTA, polyvinyl alcohol, carbon black, initiator, inhibitor and surfactant at a temperature of 50°C, a time of 2 hours and a power of 300W, the mixture is transferred to a reactor for high-temperature reaction at a temperature of 80°C and a time of 6 hours. After cooling, the mixture is stored at a low temperature.

[0122] Example 4

[0123] The environmentally friendly heat-curing impregnating agent comprises the following raw materials in parts by weight:

[0124] Triethylene glycol dimethacrylate: 70 parts;

[0125] Vinyl tris(trimethylsiloxy)silane: 65 parts;

[0126] EDTA: 15 parts;

[0127] Polyvinyl alcohol: 10 parts;

[0128] Carbon black: 10 parts;

[0129] Initiator: 10 parts;

[0130] Inhibitor: 10 parts;

[0131] Surfactant: 5 parts.

[0132] The parameters of the environmentally friendly heat-curing impregnating agent and the triethylene glycol dimethacrylate are as follows: CAS No. 109-16-0, density 1.063 g / cm 3 ;

[0133] The parameters of the vinyl tris(trimethylsiloxy)silane are as follows: CAS No. 5356-84-3, density 0.861 g / mL.

[0134] The environmentally friendly heat-curing impregnating agent, the initiator is benzoyl peroxide;

[0135] The inhibitor is 2,6-dibutyl-p-cresol;

[0136] The surfactant is cocamidopropyl betaine.

[0137] The method for preparing the environmentally friendly heat-curing impregnating agent as described above comprises the following steps:

[0138] After ultrasonically mixing triethylene glycol dimethacrylate, vinyl tri(trimethylsiloxy)silane, EDTA, polyvinyl alcohol, carbon black, initiator, inhibitor and surfactant at a temperature of 60°C, a time of 6 hours and a power of 600W, the mixture is transferred to a reactor for high-temperature reaction at a temperature of 95°C and a time of 12 hours. After cooling, the mixture is stored at a low temperature.

[0139] Example 5

[0140] The environmentally friendly heat-curing impregnating agent comprises the following raw materials in parts by weight:

[0141] Triethylene glycol dimethacrylate: 65 parts;

[0142] Vinyl tris(trimethylsiloxy)silane: 75 parts;

[0143] EDTA: 13 parts;

[0144] Polyvinyl alcohol: 15 parts;

[0145] Carbon black: 6 parts;

[0146] Initiator: 15 parts;

[0147] Inhibitor: 8 parts;

[0148] Surfactant: 10 parts.

[0149] The parameters of the environmentally friendly heat-curing impregnating agent and the triethylene glycol dimethacrylate are as follows: CAS No. 109-16-0, density 1.063 g / cm 3 ;

[0150] The parameters of the vinyl tris(trimethylsiloxy)silane are as follows: CAS No. 5356-84-3, density 0.861 g / mL.

[0151] The environmentally friendly heat-curing impregnating agent, the initiator is diisopropyl peroxydicarbonate;

[0152] The inhibitor is butylated hydroxytoluene;

[0153] The surfactant is alkylphenol polyoxyethylene ether.

[0154] The method for preparing the environmentally friendly heat-curing impregnating agent as described above comprises the following steps:

[0155] After ultrasonically mixing triethylene glycol dimethacrylate, vinyl tri(trimethylsiloxy)silane, EDTA, polyvinyl alcohol, carbon black, initiator, inhibitor and surfactant at a temperature of 55°C, a time of 4 hours and a power of 450W, the mixture is transferred to a reactor for high-temperature reaction at a temperature of 90°C and a time of 8 hours. After cooling, the mixture is stored at a low temperature.

[0156] Comparative Example 1

[0157] The environmentally friendly heat-curing impregnating agent comprises the following raw materials in parts by weight:

[0158] (Meth)acrylate: 65 parts;

[0159] Vinyl tris(trimethylsiloxy)silane: 75 parts;

[0160] EDTA: 13 parts;

[0161] Polyvinyl alcohol: 15 parts;

[0162] Carbon black: 6 parts;

[0163] Initiator: 15 parts;

[0164] Inhibitor: 8 parts;

[0165] Surfactant: 10 parts.

[0166] The parameters of the environmentally friendly heat-curing impregnating agent and the vinyl tris(trimethylsiloxy)silane are as follows: CA S No. 5356-84-3, density 0.861 g / mL.

[0167] The environmentally friendly heat-curing impregnating agent, the initiator is diisopropyl peroxydicarbonate;

[0168] The inhibitor is butylated hydroxytoluene;

[0169] The surfactant is alkylphenol polyoxyethylene ether.

[0170] The method for preparing the environmentally friendly heat-curing impregnating agent as described above comprises the following steps:

[0171] After ultrasonically mixing (meth)acrylate, vinyl tris(trimethylsiloxy)silane, EDTA, polyvinyl alcohol, carbon black, initiator, inhibitor and surfactant at a temperature of 55°C, a time of 4 hours and a power of 450W, the mixture is transferred to a reactor for high-temperature reaction at a temperature of 90°C and a time of 8 hours. After cooling, the mixture is stored at a low temperature.

[0172] Comparative Example 2

[0173] The environmentally friendly heat-curing impregnating agent comprises the following raw materials in parts by weight:

[0174] Trimethylolpropane ester: 65 parts;

[0175] Vinyl tris(trimethylsiloxy)silane: 75 parts;

[0176] EDTA: 13 parts;

[0177] Polyvinyl alcohol: 15 parts;

[0178] Carbon black: 6 parts;

[0179] Initiator: 15 parts;

[0180] Inhibitor: 8 parts;

[0181] Surfactant: 10 parts.

[0182] The parameters of the environmentally friendly heat-curing impregnating agent and the vinyl tris(trimethylsiloxy)silane are as follows: CA S No. 5356-84-3, density 0.861 g / mL.

[0183] The environmentally friendly heat-curing impregnating agent, the initiator is diisopropyl peroxydicarbonate;

[0184] The inhibitor is butylated hydroxytoluene;

[0185] The surfactant is alkylphenol polyoxyethylene ether.

[0186] The method for preparing the environmentally friendly heat-curing impregnating agent as described above comprises the following steps:

[0187] After ultrasonically mixing trimethylolpropane ester, vinyl tri(trimethylsiloxy)silane, EDTA, polyvinyl alcohol, carbon black, initiator, inhibitor and surfactant at a temperature of 55°C, a time of 4 hours and a power of 450W, the mixture is transferred to a reactor for high-temperature reaction at a temperature of 90°C and a time of 8 hours. After cooling, the mixture is stored at a low temperature.

[0188] Comparative Example 3

[0189] The environmentally friendly heat-curing impregnating agent comprises the following raw materials in parts by weight:

[0190] Triethylene glycol dimethacrylate: 65 parts;

[0191] Styryltrimethoxysilane: 75 parts;

[0192] EDTA: 13 parts;

[0193] Polyvinyl alcohol: 15 parts;

[0194] Carbon black: 6 parts;

[0195] Initiator: 15 parts;

[0196] Inhibitor: 8 parts;

[0197] Surfactant: 10 parts.

[0198] The parameters of the environmentally friendly heat-curing impregnating agent and the triethylene glycol dimethacrylate are as follows: CAS No. 109-16-0, density 1.063 g / cm 3 .

[0199] The environmentally friendly heat-curing impregnating agent, the initiator is diisopropyl peroxydicarbonate;

[0200] The inhibitor is butylated hydroxytoluene;

[0201] The surfactant is alkylphenol polyoxyethylene ether.

[0202] The method for preparing the environmentally friendly heat-curing impregnating agent as described above comprises the following steps:

[0203] After ultrasonically mixing triethylene glycol dimethacrylate, styryltrimethoxysilane, EDTA, polyvinyl alcohol, carbon black, initiator, inhibitor and surfactant at a temperature of 55°C, a time of 4 hours and a power of 450W, the mixture is transferred to a reactor for high-temperature reaction at a temperature of 90°C and a time of 8 hours. After cooling, the mixture is stored at a low temperature.

[0204] Comparative Example 4

[0205] The environmentally friendly heat-curing impregnating agent comprises the following raw materials in parts by weight:

[0206] Triethylene glycol dimethacrylate: 65 parts;

[0207] Vinyl tris(trimethylsiloxy)silane: 75 parts;

[0208] EDTA: 13 parts;

[0209] Carbon black: 6 parts;

[0210] Initiator: 15 parts;

[0211] Inhibitor: 8 parts;

[0212] Surfactant: 10 parts.

[0213] The parameters of the environmentally friendly heat-curing impregnating agent and the triethylene glycol dimethacrylate are as follows: CAS No. 109-16-0, density 1.063 g / cm 3 ;

[0214] The parameters of the vinyl tris(trimethylsiloxy)silane are as follows: CAS No. 5356-84-3, density 0.861 g / mL.

[0215] The environmentally friendly heat-curing impregnating agent, the initiator is diisopropyl peroxydicarbonate;

[0216] The inhibitor is butylated hydroxytoluene;

[0217] The surfactant is alkylphenol polyoxyethylene ether.

[0218] The method for preparing the environmentally friendly heat-curing impregnating agent as described above comprises the following steps:

[0219] After ultrasonically mixing triethylene glycol dimethacrylate, vinyl tri(trimethylsiloxy)silane, EDTA, carbon black, initiator, inhibitor and surfactant at a temperature of 55°C, a time of 4 hours and a power of 450W, the mixture is transferred to a reactor for high-temperature reaction at a temperature of 90°C and a time of 8 hours. After cooling, the mixture is stored at a low temperature.

[0220] Comparative Example 5

[0221] The environmentally friendly heat-curing impregnating agent comprises the following raw materials in parts by weight:

[0222] Triethylene glycol dimethacrylate: 65 parts;

[0223] Vinyl tris(trimethylsiloxy)silane: 75 parts;

[0224] Polyvinyl alcohol: 15 parts;

[0225] Carbon black: 6 parts;

[0226] Initiator: 15 parts;

[0227] Inhibitor: 8 parts;

[0228] Surfactant: 10 parts.

[0229] The parameters of the environmentally friendly heat-curing impregnating agent and the triethylene glycol dimethacrylate are as follows: CAS No. 109-16-0, density 1.063 g / cm 3 ;

[0230] The parameters of the vinyl tris(trimethylsiloxy)silane are as follows: CAS No. 5356-84-3, density 0.861 g / mL.

[0231] The environmentally friendly heat-curing impregnating agent, the initiator is diisopropyl peroxydicarbonate;

[0232] The inhibitor is butylated hydroxytoluene;

[0233] The surfactant is alkylphenol polyoxyethylene ether.

[0234] The method for preparing the environmentally friendly heat-curing impregnating agent as described above comprises the following steps:

[0235] After ultrasonically mixing triethylene glycol dimethacrylate, vinyl tri(trimethylsiloxy)silane, polyvinyl alcohol, carbon black, initiator, inhibitor and surfactant at a temperature of 55°C, a time of 4 hours and a power of 450W, the mixture is transferred to a reactor for high-temperature reaction at a temperature of 90°C and a time of 8 hours. After cooling, the mixture is stored at a low temperature.

[0236] Test Case

[0237] Select the impregnation agent prepared in Example 5, from Figure 1 It can be seen that the material appears as a black viscous liquid.

[0238] The impregnants prepared in Examples 1-5 and Comparative Examples 1-5 were selected for graphite bipolar plate test pieces (Toyo Graphite, isem-8, EDM electrode), and the reference method was "Chinese Invention Patent, Publication No.: CN118006249A". The test method for volume shrinkage was tested with reference to the density method in GB / T 24148.9-2014. The test method for the hardness of the solidified material was tested with reference to the Shore durometer method specified in GB / T 2411. The test method for the first-time sizing pass rate was tested with reference to the standard test piece method specified in HG / T6100-2022. 50 typical graphite pressing test pieces were made in each group, and water tests were carried out under an air pressure of 0.33MPa. The leakage level was ≤2 and qualified.

[0239] Table 1 Test results

[0240]

[0241] As shown in Table 1, in general, the impregnant prepared by the embodiment of the present invention is superior to the impregnant prepared by the comparative example as a whole and has better mechanical properties. After analysis as follows, the replacement of triethylene glycol dimethacrylate with (meth) acrylate in comparative example 1 and the replacement of triethylene glycol dimethacrylate with (meth) acrylate in comparative example 1 are important chemical substitutions, which affect the performance of the impregnant, especially its high temperature resistance. The mechanism of this substitution is analyzed from the perspective of chemical structure and properties. The main difference between triethylene glycol dimethacrylate and (meth) acrylate lies in their structure. Since triethylene glycol dimethacrylate contains a triethylene glycol moiety, this means that it contains a longer alkoxy chain, and such a structure provides better stability at high temperatures. On the contrary, (meth) acrylate has a simpler structure and no long alkoxy chain, so its high temperature resistance is not as good as triethylene glycol dimethacrylate. From a thermodynamic point of view, longer alkoxy chains in molecules can increase the intermolecular forces of molecules, thereby improving their thermal stability. Because of its long alkoxy chain, triethylene glycol dimethacrylate naturally has a larger intermolecular force, which makes it more difficult to decompose or react under high temperature conditions, thereby showing good high temperature resistance. Due to its complex structure, triethylene glycol dimethacrylate has a lower reactivity than (meth) acrylate, which also means that it is less likely to undergo chemical changes under high temperature conditions, which proves its good high temperature resistance from another aspect. Triethylene glycol dimethacrylate is used to prepare an environmentally friendly thermosetting impregnant, and its excellent high temperature resistance enables this impregnant to remain stable at a higher operating temperature, thereby improving the repair effect and durability of mechanical parts. On the contrary, the impregnant using (meth) acrylate has poor high temperature resistance and performance degradation in high temperature applications. In general, replacing triethylene glycol dimethacrylate with (meth) acrylate in Comparative Example 1 will result in a decrease in the high temperature resistance of the prepared impregnant, which is mainly due to the difference in thermal stability and chemical reactivity caused by the chemical structure differences of the two compounds. Therefore, triethylene glycol dimethacrylate is more suitable for application environments that require high temperature resistance. Comparative Example 2 replaces triethylene glycol dimethacrylate with trimethylolpropane ester. In Comparative Example 2, triethylene glycol dimethacrylate is replaced by trimethylolpropane ester. This replacement mainly affects the water resistance of the impregnant. From the perspective of chemical structure and properties, the following is the mechanism by which this replacement affects the performance of the environmentally friendly thermosetting impregnant: The main structural differences between triethylene glycol dimethacrylate and trimethylolpropane ester are the chemical skeleton and functional groups. Triethylene glycol dimethacrylate contains a longer alkoxy chain and acrylate functional groups, while trimethylolpropane ester contains three hydroxyl (-OH) functional groups in its structure. Hydroxyl groups are more likely to form stronger interactions with water molecules through hydrogen bonds due to their strong polarity.Since the hydroxyl groups in trimethylolpropane ester have strong polarity and the ability to form hydrogen bonds with water molecules, the introduction of this structure helps to improve the water resistance of environmentally friendly thermosetting impregnants. When the impregnant is exposed to a humid or water environment, the interaction between the hydroxyl groups in trimethylolpropane ester and water molecules can reduce the penetration and influence of water molecules in the impregnant, thereby improving its overall water resistance. The introduction of hydroxyl groups not only affects water resistance, but also changes some physical properties of the impregnant, such as viscosity and mechanical strength. Compared with triethylene glycol dimethacrylate, trimethylolpropane ester will cause changes in the viscosity and crosslinking density of the impregnant due to its structural characteristics, which in turn affects the mechanical properties of the final product. Improving the water resistance of the impregnant is extremely important for some specific application environments, especially those that are exposed to moisture or direct contact with water. Therefore, using trimethylolpropane ester to replace triethylene glycol dimethacrylate can broaden the application range and market potential of the impregnant to a certain extent. In summary, the purpose of replacing triethylene glycol dimethacrylate with trimethylolpropane ester is mainly to improve the water resistance of the impregnant. This replacement is achieved by enhancing the interaction between the impregnant and the water molecules, and at the same time affects some of the physical properties of the impregnant, thereby having a positive impact on its application performance and scope. Comparative Example 3 replaces vinyl tris (trimethylsiloxane) silane with styryl trimethoxy silane. In Comparative Example 3, vinyl tris (trimethylsiloxane) silane is replaced with styryl trimethoxy silane. This replacement affects the corrosion resistance and interaction mechanism of the impregnant. The following is an analysis of the impact mechanism of this replacement from the perspective of chemical structure and properties: The main difference between vinyl tris (trimethylsiloxane) silane and styryl trimethoxy silane is the functional group at the end of the silane, vinyl (-CH=CH2) and benzene ring (C6H5-). Due to the introduction of the benzene ring structure, styryl trimethoxy silane exhibits higher rigidity and thermal stability. In addition, the presence of benzene rings can also improve the chemical resistance of the material, because benzene rings have strong aromaticity and can resist corrosion from a variety of chemicals. The use of styryltrimethoxysilane in the impregnant improves its corrosion resistance. The benzene ring structure is not easy to react with the surrounding chemicals, providing better chemical stability for the impregnant. This makes the impregnant more suitable for environments with harsh chemical properties, such as the presence of corrosive substances such as acids and alkalis. Compared with vinyl, the introduction of benzene rings changes the interaction mechanism between silane and the substrate. Due to the rigidity and hydrophobicity of the benzene ring, styryltrimethoxysilane interacts with the substrate surface in different ways, thereby affecting the adhesion and dispersibility of the impregnant. This change has the effect of further enhancing the overall performance of the material, especially in applications that require good interfacial compatibility. The introduction of aromatic benzene ring structures can also improve the thermal stability of the impregnant. The aromatic structure of the benzene ring has a strong ability to absorb heat energy, allowing styryltrimethoxysilane to maintain better chemical stability in high temperature environments.This feature is particularly suitable for applications that require working at high temperatures. In general, the replacement with styryltrimethoxysilane can improve the corrosion resistance and thermal stability of environmentally friendly heat-curing impregnants. This replacement not only takes advantage of the chemical stability of the benzene ring, but also optimizes the overall performance of the material by changing the interaction mode with the substrate, providing a wider range of applications for the impregnant. Comparative Example 4 removes polyvinyl alcohol. The removal of polyvinyl alcohol (PVA) in Comparative Example 4 involves an important formulation adjustment, which has a direct impact on the final performance of the environmentally friendly heat-curing impregnant. Polyvinyl alcohol is widely used in a variety of material systems, mainly due to its excellent film-forming properties, adhesion and water solubility. The following is an analysis of the impact mechanism of removing polyvinyl alcohol from a chemical and physical perspective: Polyvinyl alcohol generally plays the role of a viscosity regulator in the formulation. Removing PVA will cause the viscosity of the impregnant to decrease, which can make it easier to penetrate into the pores of parts such as castings, weldments and die-castings, but it also reduces the load of the impregnant, affecting the durability and stability of the repair effect. PVA is used in the impregnant formulation because of its excellent film-forming properties, and can form a uniform and continuous film layer. After removing PVA, it is difficult for the impregnant to form a complete and uniform protective layer on the repaired surface, affecting its protective effect on the surface of the repaired part. The water solubility of PVA makes it easy to use and clean the impregnant based on it in an aqueous environment. Removing PVA reduces the water solubility of the impregnant, which affects the convenience and cleanliness of the operation to a certain extent. PVA has good adhesion and can enhance the bonding strength between the impregnant and the material. Impregnants without PVA will have a decrease in adhesion performance, which will affect the uniformity and durability of the repair effect. Although removing polyvinyl alcohol can lead to some of the above-mentioned negative effects, it also brings some potential benefits, such as cost savings (due to reduced material input) and improved rheological properties (better penetration effect). Therefore, it is crucial to weigh the use of PVA according to specific application scenarios and performance requirements. In the case of removing PVA, it is necessary to compensate or improve the overall performance of the impregnant by optimizing the proportion of other components or introducing new additives. Comparative Example 5 removes EDTA. Removing EDTA (ethylenediaminetetraacetic acid) in Comparative Example 5 will have a direct impact on the performance of the environmentally friendly thermosetting impregnant. EDTA is a widely used chelating agent that forms stable complexes with a variety of metal ions. The following is an analysis of the impact of removing EDTA from a chemical and performance perspective: One of the main functions of EDTA is to chelate metal ions to prevent these ions from catalyzing unintended chemical reactions that lead to premature curing or performance degradation. After EDTA is removed, metal ions (such as iron, copper, etc.) in the impregnant will accelerate certain reactions, such as the decomposition of the initiator, resulting in reduced storage stability and service life. EDTA can also reduce material corrosion by chelating ions on the metal surface. Without EDTA, metal surfaces are more susceptible to corrosion under certain conditions, especially in high humidity environments.EDTA also acts as a buffer in some systems, helping to maintain a stable pH in the formulation. Removing EDTA causes fluctuations in pH, which in turn affects the overall stability and performance of the infiltrant. In special environments containing heavy metal ions, the chelating effect of EDTA can prevent these ions from negatively affecting the performance of the infiltrant. In the absence of EDT A, these heavy metal ions can interfere with the curing process or reduce the quality of the repair. Although removing EDTA reduces material costs and contributes to environmental friendliness (because EDTA and its metal complexes are slowly biodegradable in the environment), other methods are needed to compensate for the above potential negative effects. This includes finding other types of stabilizers or chelators to replace the function of EDTA, or by adjusting the concentrations of other components in the formulation to maintain the desired performance and stability. In short, when considering removing EDTA, it is necessary to carefully consider its multi-faceted impact on the performance of the final product and evaluate whether other ingredients need to be introduced to supplement or improve these properties.

[0242] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. An environmentally friendly thermosetting impregnant, characterized in that: In parts by weight, the following raw materials are included: Triethylene glycol dimethacrylate: 50-80 parts; Vinyl tris(trimethylsiloxy)silane: 60-90 parts; EDTA: 10-20 parts; Polyvinyl alcohol: 10-25 parts; Carbon black: 2-10 parts; Initiator: 10-20 parts; Inhibitor: 2-10 parts; Surfactant: 5-15 parts.

2. The environmentally friendly heat-curing impregnating agent according to claim 1, characterized in that: In parts by weight, the following raw materials are included: Triethylene glycol dimethacrylate: 55-70 parts; Vinyl tris(trimethylsiloxy)silane: 65-80 parts; EDTA: 10-15 parts; Polyvinyl alcohol: 10-20 parts; Carbon black: 2-10 parts; Initiator: 10-20 parts; Inhibitor: 2-10 parts; Surfactant: 5-15 parts.

3. The environmentally friendly heat-curing impregnating agent according to claim 2, characterized in that: In parts by weight, the following raw materials are included: Triethylene glycol dimethacrylate: 65 parts; Vinyl tris(trimethylsiloxy)silane: 75 parts; EDTA: 13 parts; Polyvinyl alcohol: 15 parts; Carbon black: 6 parts; Initiator: 15 parts; Inhibitor: 8 parts; Surfactant: 10 parts.

4. The environmentally friendly heat-curing impregnating agent according to claim 3, characterized in that: The parameters of triethylene glycol dimethacrylate are as follows: CAS No. 109-16-0, density 1.063 g / cm 3 ; The parameters of the vinyl tris(trimethylsiloxy)silane are as follows: CAS No. 5356-84-3, density 0.861 g / mL.

5. The environmentally friendly heat-curing impregnating agent according to claim 3, characterized in that: The initiator is diisopropyl peroxydicarbonate or benzoyl peroxide; The inhibitor is one of sodium pyrosulfite, tert-butylquinone, dibutylhydroxytoluene, and 2,6-dibutyl-p-cresol; The surfactant is one of polysorbate, alkylphenol polyoxyethylene ether, tetraalkylammonium chloride, sodium lauryl sulfate and cocamidopropyl betaine.

6. A method for preparing the environmentally friendly heat-curing impregnating agent according to claim 1, characterized in that: The following steps are involved: After ultrasonically mixing triethylene glycol dimethacrylate, vinyl tri(trimethylsiloxy)silane, EDTA, polyvinyl alcohol, carbon black, initiator, inhibitor and surfactant, the mixture is transferred to a reaction kettle for high-temperature reaction, cooled and then stored at low temperature.

7. The method for preparing the environmentally friendly heat-curing impregnating agent according to claim 6, characterized in that: The temperature of ultrasonic mixing is 50℃-60℃; The ultrasonic mixing time is 2h-6h; The power of ultrasonic mixing is 300W-600W.

8. The method for preparing the environmentally friendly heat-curing impregnating agent according to claim 6, characterized in that: The temperature of the high temperature reaction is 80℃-95℃; The high temperature reaction time is 6h-12h.