Novel quaternization side chain type anion exchange membrane

By using components such as sulfonated polyether ether ketone and quaternary ammonium salt groups in the anion exchange membrane, the quaternary side chain anion exchange membrane is solved, and the existing membranes have been solved in the ion exchange capacity, conductivity, mechanical properties and The problem of insufficient chemical stability achieves higher performance and wider application applicability.

CN118909388APending Publication Date: 2024-11-08山西国润储能科技有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410975935.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing anion exchange membranes have shortcomings in ion exchange capacity, conductivity, mechanical properties and chemical stability, which limits their application in high-efficiency energy conversion and industrial processing.

Method used

60%-80% sulfonated polyether ether ketone, 10%-20% side chain monomer containing two quaternary ammonium groups, 5%-10% crosslinking agent, 1%-3% A mixture of catalyst, 2%-5% toughening agent and an appropriate amount of solvent is formed by heat treatment to form a quaternized side chain anion exchange membrane.

Benefits of technology

It significantly improves the ion exchange capacity, conductivity and mechanical properties, enhances chemical stability, and keeps the membrane stable under high stress and strong alkaline environments. It is suitable for a variety of industrial and energy applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118909388A_ABST
    Figure CN118909388A_ABST
Patent Text Reader

Abstract

The invention relates to the field of ion exchange materials, and discloses a novel quaternization side chain type anion exchange membrane. The anion exchange membrane comprises a mixture of the following components: 60%-80% of sulfonated polyetheretherketone, 10%-20% of a side chain monomer containing two quaternary ammonium salt groups, 5%-10% of a cross-linking agent, 1%-3% of a catalyst, 2%-5% of a flexibilizer and a proper amount of a solvent for dissolving and dispersing the components. According to the anion exchange membrane, side chain monomers containing two quaternary ammonium salt groups are introduced, so that ion exchange sites are remarkably increased, the higher ion exchange capacity is provided and reaches 1.5-3.5 meq / g, due to the characteristic, the membrane can efficiently carry out anion exchange in application of flow batteries, fuel cells, electrolyzed water and the like, the ion exchange efficiency and effect are improved, and the service life of the membrane is prolonged. The introduction of the quaternary ammonium salt group optimizes the transmission channel of anions and reduces the ion migration resistance, thereby enhancing the conductivity of the membrane.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of ion exchange materials, in particular to a novel quaternary ammonium side chain type anion exchange membrane. Background Art

[0002] With the continuous growth of modern industry and energy demand, the application of ion exchange membranes in fuel cells, water electrolysis, flow batteries and other fields has become increasingly important. These applications have put forward higher requirements on the ion exchange capacity, conductivity, mechanical properties and chemical stability of anion exchange membranes. However, the existing anion exchange membranes still have many shortcomings in performance, which limits their wide application in efficient energy conversion and industrial processing. Therefore, the development of a new anion exchange membrane with excellent performance and strong adaptability has become a hot spot and difficulty in current research.

[0003] Anion exchange membranes are formed by introducing quaternary ammonium salt groups into polymer substrates and are widely used in the fields of fuel cells, water electrolysis and flow batteries. However, anion exchange membranes in the prior art still have the following significant deficiencies:

[0004] Insufficient ion exchange capacity:

[0005] The number of ion exchange sites in conventional anion exchange membranes is limited, and the ion exchange capacity is usually below 1.0 meq / g. This low capacity limits the application of the membrane in efficient ion exchange processes, making it perform poorly in applications that require high ion exchange capacity, such as wastewater treatment and fuel cells.

[0006] Low conductivity:

[0007] The conductivity of existing anion exchange membranes is usually around 1×10 -3 Up to 1×10 -2 S / cm, which cannot meet the requirements of efficient energy conversion devices. The unreasonable design of ion transport channels leads to large ion migration resistance, which limits the performance of the membrane in high conductivity applications. This poses an obstacle to improving the overall performance of fuel cells and electrolysis devices.

[0008] Poor mechanical properties:

[0009] Many existing anion exchange membranes are insufficient in terms of mechanical properties, especially under conditions of high stress and frequent deformation, and are prone to rupture or damage. Traditional membrane materials have poor flexibility and durability, short service life, and high maintenance costs, which affect their economic benefits and widespread application.

[0010] Poor chemical stability:

[0011] Existing anion exchange membranes are easily degraded in a strong alkaline environment and have poor chemical stability. This deficiency makes it difficult for the membrane to operate stably for a long time in a highly corrosive industrial environment, affecting the reliability and safety of the system and limiting its applicability in a variety of industrial applications.

[0012] In summary, existing anion exchange membranes have obvious deficiencies in ion exchange capacity, conductivity, mechanical properties and chemical stability. It is urgent to develop a new type of high-performance anion exchange membrane to meet the needs of modern industrial and energy applications. Summary of the invention

[0013] In view of the deficiencies of the prior art, the present invention provides a novel quaternary ammonium side chain anion exchange membrane, which solves the problems existing in the traditional anion exchange membrane in terms of ion exchange capacity, conductivity, mechanical properties and chemical stability.

[0014] To achieve the above objectives, the present invention is implemented by the following technical scheme: a novel quaternary ammonium side chain anion exchange membrane, the anion exchange membrane comprises a mixture of the following components:

[0015] 60%-80% sulfonated polyetheretherketone;

[0016] 10%-20% of a side chain monomer containing two quaternary ammonium salt groups;

[0017] 5%-10% cross-linking agent;

[0018] 1%-3% catalyst;

[0019] 2%-5% toughening agent;

[0020] An appropriate amount of solvent is used to dissolve and disperse the components.

[0021] Preferably, the side chain monomer is an allyl compound containing two tetramethylammonium hydroxide groups.

[0022] Preferably, the sulfonation degree of the sulfonated polyetheretherketone is between 20% and 60%.

[0023] Preferably, the crosslinking agent is divinylbenzene or divinylphenyl phosphate.

[0024] Preferably, the catalyst is benzoyl peroxide or dicumyl peroxide; the solvent is N,N-dimethylformamide, N,N-dimethylacetamide, N-methylpyrrolidone or dimethyl sulfoxide.

[0025] Preferably, the toughening agent is one or more of polyethylene glycol, ethylene glycol dimethyl ether, and polyethylene oxide.

[0026] Preferably, a novel method for preparing a quaternary ammonium side chain anion exchange membrane comprises the following steps:

[0027] Dissolve sulfonated polyetheretherketone in a suitable amount of solvent;

[0028] Add a side chain monomer containing two quaternary ammonium salt groups to the solution and stir thoroughly;

[0029] Add cross-linking agent and catalyst, and continue stirring until uniform;

[0030] Add toughening agent and stir evenly;

[0031] The obtained mixture is poured into a mold to form a film;

[0032] The anion exchange membrane is obtained by heat treatment at an appropriate temperature to remove the solvent.

[0033] Preferably, the solution is stirred for 2-4 hours; the heat treatment temperature is 80-120° C. and the time is 4-8 hours.

[0034] Preferably, the ion exchange capacity of the anion exchange membrane is between 1.5 and 3.5 meq / g; the conductivity of the anion exchange membrane is between 1×10 -2 Up to 5×10 -1 S / cm.

[0035] The present invention provides a novel quaternary ammonium side chain anion exchange membrane having the following beneficial effects:

[0036] 1. The anion exchange membrane significantly increases the ion exchange sites by introducing side chain monomers containing two quaternary ammonium salt groups, providing a higher ion exchange capacity of 1.5 to 3.5 meq / g. This feature enables the membrane to efficiently exchange anions in applications such as flow batteries, fuel cells, and water electrolysis, improving the efficiency and effect of ion exchange.

[0037] 2. The anion exchange membrane of the present invention has excellent performance in high conductivity, reaching 1×10 -2 Up to 5×10 -1 S / cm. The introduction of quaternary ammonium salt groups optimizes the transmission channels of anions, reduces the resistance to ion migration, and thus improves the conductivity of the membrane. This is particularly important for the application of fuel cells, flow batteries, and electrolysis devices, and can significantly improve the energy conversion efficiency and overall performance of the system.

[0038] 3. The addition of toughening agent in the anion exchange membrane of the present invention significantly improves the mechanical properties of the membrane, making it have good durability and flexibility. The membrane can maintain structural integrity under high stress and frequent deformation conditions, is not easy to break or damage, prolongs the service life, reduces the frequency of maintenance and replacement, and improves economic benefits.

[0039] 4. The present invention uses sulfonated polyetheretherketone as the substrate, which gives the membrane excellent chemical stability, especially in a strong alkaline environment, and is not easy to degrade. This feature ensures that the membrane can operate stably for a long time in a highly corrosive industrial environment, improves the reliability and safety of the system, and is suitable for a variety of industrial applications. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] Figure 1 The present invention is a flow chart of the preparation method of a novel quaternary ammonium side chain anion exchange membrane. DETAILED DESCRIPTION

[0041] The following will be combined with the drawings in the specification of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0042] Example:

[0043] Please see attached Figure 1 :

[0044] Example 1: Highly sulfonated polyetheretherketone membrane

[0045] step:

[0046] 70% sulfonated polyetheretherketone (sulfonation degree 60%) was dissolved in N,N-dimethylformamide (DMF) and stirred for 2 hours.

[0047] 15% of an allyl compound containing two tetramethylammonium hydroxide groups was added to the solution and stirred for 1 hour.

[0048] 7% of divinylbenzene and 2% of benzoyl peroxide were added and stirring was continued for 30 minutes.

[0049] Add 3% polyethylene glycol and stir well.

[0050] The mixture is poured into a mold to form a film.

[0051] The solvent was removed by heat treatment at 100°C for 6 hours to obtain an anion exchange membrane.

[0052] Summary: This example improves the ion exchange capacity by using sulfonated polyetheretherketone with a high degree of sulfonation. The obtained membrane exhibits excellent conductivity and chemical stability and is suitable for high-performance fuel cell applications.

[0053] Example 2: Toughened anion exchange membrane

[0054] step:

[0055] 65% sulfonated polyetheretherketone (sulfonation degree 40%) was dissolved in N,N-dimethylformamide (DMF) and stirred for 3 hours.

[0056] 12% of an allyl compound containing two tetramethylammonium hydroxide groups was added to the solution and stirred for 1 hour.

[0057] 8% of divinylphenyl phosphate and 2% of dicumyl peroxide were added and stirring was continued for 30 minutes.

[0058] Add 5% of ethylene glycol dimethyl ether and stir well.

[0059] The mixture is poured into a mold to form a film.

[0060] The solvent was removed by heat treatment at 90°C for 4 hours to obtain an anion exchange membrane.

[0061] Summary: In this example, the mechanical properties of the membrane were improved by adding ethylene glycol dimethyl ether toughening agent, and the obtained membrane had good flexibility and durability and was suitable for liquid flow batteries.

[0062] Example 3: High conductivity anion exchange membrane

[0063] step:

[0064] 60% sulfonated polyetheretherketone (sulfonation degree 30%) was dissolved in N,N-dimethylformamide (DMF) and stirred for 2.5 hours.

[0065] To the solution was added 20% of an allyl compound containing two tetramethylammonium hydroxide groups and stirred for 1 hour.

[0066] 5% of divinylbenzene and 2% of benzoyl peroxide were added and stirring was continued for 40 minutes.

[0067] Add 3% polyethylene oxide and stir well.

[0068] The mixture is poured into a mold to form a film.

[0069] The reaction mixture was heat treated at 80°C for 8 hours to remove the solvent, thereby obtaining an anion exchange membrane.

[0070] Summary: This embodiment significantly improves the conductivity of the membrane by increasing the content of quaternary ammonium salt groups, so that it exhibits excellent energy conversion efficiency in the electrolysis device.

[0071] Example 4: Low sulfonation degree sulfonated polyetheretherketone membrane

[0072] step:

[0073] 75% of sulfonated polyetheretherketone (sulfonation degree 20%) was dissolved in N,N-dimethylformamide (DMF) and stirred for 3 hours.

[0074] To the solution was added 10% of an allyl compound containing two tetramethylammonium hydroxide groups and stirred for 1 hour.

[0075] 8% of divinylphenyl phosphate and 1% of dicumyl peroxide were added and stirring was continued for 20 minutes.

[0076] Add 5% polyethylene glycol and stir well.

[0077] The mixture is poured into a mold to form a film.

[0078] The solvent was removed by heat treatment at 110°C for 5 hours to obtain an anion exchange membrane.

[0079] Summary: This embodiment improves the chemical stability of the membrane by reducing the degree of sulfonation, and is suitable for applications in strong alkaline environments, such as industrial water electrolysis equipment.

[0080] Example 5: Optimized anion exchange membrane

[0081] step:

[0082] 70% sulfonated polyetheretherketone (sulfonation degree 50%) was dissolved in N,N-dimethylformamide (DMF) and stirred for 2 hours.

[0083] 15% of an allyl compound containing two tetramethylammonium hydroxide groups was added to the solution and stirred for 1 hour.

[0084] 7% of divinylbenzene and 2% of benzoyl peroxide were added and stirring was continued for 30 minutes.

[0085] Add 3% polyethylene glycol and stir well.

[0086] The mixture is poured into a mold to form a film.

[0087] The solvent was removed by heat treatment at 90°C for 6 hours to obtain an anion exchange membrane.

[0088] Summary: This embodiment achieves a good balance of ion exchange capacity, conductivity, mechanical properties and chemical stability by optimizing the ratio of each component, and is suitable for a variety of application scenarios, including fuel cells and wastewater treatment.

[0089] Summary of Examples

[0090] The five embodiments of the present invention demonstrate quaternary ammonium side chain anion exchange membranes prepared under different formulations and process conditions, highlighting the following key points:

[0091] High ion exchange capacity: Examples 1 and 5 improve the ion exchange capacity by using sulfonated polyetheretherketone with different sulfonation degrees, so that they perform well in high-efficiency ion exchange applications.

[0092] Excellent electrical conductivity: Example 3 significantly improves electrical conductivity by increasing the content of quaternary ammonium salt groups, which is suitable for the high energy conversion efficiency requirements in electrolysis devices.

[0093] Good mechanical properties: Example 2 and Example 5 significantly improve the mechanical properties of the membrane and extend the service life by adding different toughening agents, and are suitable for working conditions with high stress and frequent deformation.

[0094] Excellent chemical stability: Example 4 improves the chemical stability of the membrane in a strong alkaline environment by reducing the degree of sulfonation, ensuring long-term stable operation in a corrosive industrial environment.

[0095] Comprehensive performance optimization: Example 5 achieves a good balance of ion exchange capacity, conductivity, mechanical properties and chemical stability by optimizing the ratio of each component, and is suitable for a variety of application scenarios.

[0096] Through the analysis of the above embodiments, the present invention provides a novel quaternary ammonium side chain anion exchange membrane, which can effectively solve the deficiencies in the prior art and meet the needs of modern industrial and energy applications.

[0097] Comparative experiment:

[0098] Experiment 1: Ion exchange capacity comparison experiment

[0099] Experimental purpose: To compare the ion exchange capacity of the anion exchange membrane of the present invention with that of the prior art membrane.

[0100] Existing technology: traditional sulfonated polyetheretherketone anion exchange membrane

[0101] Composition: 70% sulfonated polyetheretherketone (sulfonation degree 30%), 20% side chain monomer of monoquaternary ammonium salt group, 7% divinylbenzene, 2% benzoyl peroxide, appropriate amount of N,N-dimethylformamide

[0102] Preparation method: dissolve the above components in a solvent, stir evenly to form a film, and heat treat at 80°C for 6 hours.

[0103] The present invention: quaternary ammonium side chain anion exchange membrane

[0104] Composition: 70% sulfonated polyetheretherketone (sulfonation degree 50%), 15% side chain monomer containing two quaternary ammonium salt groups, 8% divinylphenyl phosphate, 2% diisopropylbenzene peroxide, 5% polyethylene glycol, and appropriate amount of N,N-dimethylformamide.

[0105] Preparation method: dissolve the above components in a solvent, stir evenly to form a film, and heat treat at 90°C for 8 hours.

[0106] Experimental steps:

[0107] The conventional sulfonated polyetheretherketone anion exchange membrane and the quaternized side chain anion exchange membrane of the present invention are prepared.

[0108] The ion exchange capacity (meq / g) of each membrane was measured using an ion exchange capacity tester (such as a potentiometric titrator).

[0109] Experimental data:

[0110] parameter Conventional anion exchange membrane Anion exchange membrane of the present invention Sulfonation degree 0.3 0.5 Quaternary ammonium salt group Single group Double group Ion exchange capacity (meq / g) 1.2 3.4

[0111] Summary: The ion exchange capacity of the anion exchange membrane of the present invention is significantly higher than that of the prior art, reaching 3.4 meq / g, which is nearly 3 times higher than 1.2 meq / g of the traditional membrane.

[0112] Experiment 2: Conductivity comparison experiment

[0113] Experimental purpose: To compare the conductivity of the anion exchange membrane of the present invention with that of the prior art membrane.

[0114] Existing technology: traditional sulfonated polyetheretherketone anion exchange membrane

[0115] Composition: 65% sulfonated polyetheretherketone (sulfonation degree 40%), 15% side chain monomer of monoquaternary ammonium salt group, 10% divinylbenzene, 2% benzoyl peroxide, 8% N,N-dimethylformamide.

[0116] Preparation method: dissolve the above components in a solvent, stir evenly to form a film, and heat treat at 85°C for 6 hours.

[0117] The present invention: quaternary ammonium side chain anion exchange membrane

[0118] Composition: 60% sulfonated polyetheretherketone (sulfonation degree 30%), 20% side chain monomer containing two quaternary ammonium salt groups, 7% divinylbenzene, 2% benzoyl peroxide, 11% polyethylene glycol, and appropriate amount of N,N-dimethylformamide.

[0119] Preparation method: dissolve the above components in a solvent, stir evenly to form a film, and heat treat at 90°C for 7 hours.

[0120] Experimental steps:

[0121] The conventional sulfonated polyetheretherketone anion exchange membrane and the quaternized side chain anion exchange membrane of the present invention are prepared.

[0122] The conductivity (S / cm) of each membrane was measured using a conductivity tester (such as an impedance analyzer).

[0123] Experimental data:

[0124] parameter Conventional anion exchange membrane Anion exchange membrane of the present invention Conductivity (S / cm) <![CDATA[1.5×10 -3 ]]> <![CDATA[4.2×10 -2 ]]>

[0125] Summary: The conductivity of the anion exchange membrane of the present invention is significantly higher than that of the prior art, reaching 4.2×10^-2S / cm, which is about 28 times higher than 1.5×10^-3S / cm of the traditional membrane.

[0126] Experiment 3: Mechanical properties comparison experiment

[0127] Experimental purpose: To compare the mechanical properties of the anion exchange membrane of the present invention with those of the prior art membrane.

[0128] Existing technology: traditional sulfonated polyetheretherketone anion exchange membrane

[0129] Composition: 68% sulfonated polyetheretherketone (sulfonation degree 35%), 15% side chain monomer of monoquaternary ammonium salt group, 10% divinylbenzene, 2% benzoyl peroxide, 5% N,N-dimethylformamide.

[0130] Preparation method: dissolve the above components in a solvent, stir evenly to form a film, and heat treat at 85°C for 5 hours.

[0131] The present invention: quaternary ammonium side chain anion exchange membrane

[0132] Composition: 65% sulfonated polyetheretherketone (sulfonation degree 50%), 15% side chain monomer containing two quaternary ammonium salt groups, 8% divinylphenyl phosphate, 2% diisopropylbenzene peroxide, 10% polyethylene glycol, and appropriate amount of N,N-dimethylformamide.

[0133] Preparation method: dissolve the above components in a solvent, stir evenly to form a film, and heat treat at 90°C for 8 hours.

[0134] Experimental steps:

[0135] The conventional sulfonated polyetheretherketone anion exchange membrane and the quaternized side chain anion exchange membrane of the present invention are prepared.

[0136] The elongation at break and the tensile strength of each film were measured using a mechanical property tester (such as a universal testing machine).

[0137] Experimental data:

[0138] parameter Conventional anion exchange membrane Anion exchange membrane of the present invention Elongation at break (%) 12 55 Tensile strength(MPa) 18 42

[0139] Summary: The mechanical properties of the anion exchange membrane of the present invention are significantly better than those of the prior art, with the elongation at break increased by 4.6 times and the tensile strength increased by 2.3 times.

[0140] Experiment 4: Chemical stability comparison experiment

[0141] Experimental purpose: To compare the chemical stability of the anion exchange membrane of the present invention with that of the prior art membrane.

[0142] Existing technology: traditional sulfonated polyetheretherketone anion exchange membrane

[0143] Composition: 70% sulfonated polyetheretherketone (sulfonation degree 40%), 15% side chain monomer of monoquaternary ammonium salt group, 8% divinylbenzene, 2% benzoyl peroxide, 5% N,N-dimethylformamide.

[0144] Preparation method: dissolve the above components in a solvent, stir evenly to form a film, and heat treat at 85°C for 6 hours.

[0145] The present invention: quaternary ammonium side chain anion exchange membrane

[0146] Composition: 70% sulfonated polyetheretherketone (sulfonation degree 50%), 15% side chain monomer containing two quaternary ammonium salt groups, 7% divinylphenyl phosphate, 2% diisopropylbenzene peroxide, 6% polyethylene glycol, and appropriate amount of N,N-dimethylformamide.

[0147] Preparation method: dissolve the above components in a solvent, stir evenly to form a film, and heat treat at 90°C for 7 hours.

[0148] Experimental steps:

[0149] The conventional sulfonated polyetheretherketone anion exchange membrane and the quaternized side chain anion exchange membrane of the present invention are prepared.

[0150] Each membrane was immersed in 1 M NaOH solution, and the ion exchange capacity and conductivity were tested after different time periods.

[0151] The performance of the membrane was measured using an ion exchange capacity tester and a conductivity tester after 0, 24, 48 and 72 hours, respectively.

[0152] Experimental data:

[0153]

[0154] In summary, the chemical stability of the anion exchange membrane of the present invention in a strong alkaline environment is significantly better than that of the prior art. The ion exchange capacity and conductivity after immersion for 72 hours are maintained at 2.9 meq / g and 3.7×10 -2 S / cm, while the traditional membranes are reduced to 0.5meq / g and 0.5×10 -3 S / cm.

[0155] Summary:

[0156] Through the above four comparative experiments, the significant advantages of the present invention over the prior art are fully demonstrated. The novel quaternized side chain anion exchange membrane of the present invention exhibits excellent performance in ion exchange capacity, conductivity, mechanical properties and chemical stability, can meet the higher requirements of modern industrial and energy applications, and has broad application prospects. Each experiment shows the technical solutions and experimental parameters of the prior art and the present invention in detail, and fully demonstrates the creativity and superiority of the present invention through comprehensive data comparison.

[0157] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A novel quaternary ammonium side chain anion exchange membrane, characterized in that: The anion exchange membrane comprises a mixture of the following components: 60%-80% sulfonated polyetheretherketone; 10%-20% of a side chain monomer containing two quaternary ammonium salt groups; 5%-10% cross-linking agent; 1%-3% catalyst; 2%-5% toughening agent; An appropriate amount of solvent is used to dissolve and disperse the components.

2. A novel quaternary ammonium side chain anion exchange membrane according to claim 1, characterized in that: The side chain monomer is an allyl compound containing two tetramethylammonium hydroxide groups.

3. A novel quaternary ammonium side chain anion exchange membrane according to claim 1, characterized in that: The sulfonation degree of the sulfonated polyetheretherketone is between 20% and 60%.

4. A novel quaternary ammonium side chain anion exchange membrane according to claim 1, characterized in that: The crosslinking agent is divinylbenzene or divinylphenyl phosphate.

5. A novel quaternary ammonium side chain anion exchange membrane according to claim 1, characterized in that: The catalyst is benzoyl peroxide and dicumyl peroxide; the solvent is N,N-dimethylformamide, N,N-dimethylacetamide, N-methylpyrrolidone and dimethyl sulfoxide.

6. A novel quaternary ammonium side chain anion exchange membrane according to claim 1, characterized in that: The toughening agent is one or more of polyethylene glycol, ethylene glycol dimethyl ether and polyethylene oxide.

7. A method for preparing a novel quaternary ammonium side chain anion exchange membrane according to any one of claims 1 to 6, characterized in that: The following steps are involved: Dissolve sulfonated polyetheretherketone in a suitable amount of solvent; Add a side chain monomer containing two quaternary ammonium salt groups to the solution and stir thoroughly; Add cross-linking agent and catalyst, and continue stirring until uniform; Add toughening agent and stir evenly; The resulting mixture is poured into a mold to form a film; The anion exchange membrane is obtained by heat treatment at an appropriate temperature to remove the solvent.

8. The method for preparing a novel quaternary ammonium side chain anion exchange membrane according to claim 7, characterized in that: The stirring time of the solution is 2-4 hours; the heat treatment temperature is 80-120° C. and the time is 4-8 hours.

9. The method for preparing a novel quaternary ammonium side chain anion exchange membrane according to claim 7, characterized in that: The ion exchange capacity of the anion exchange membrane is between 1.5 and 3.5 meq / g; the conductivity of the anion exchange membrane is between 1×10 -2 Up to 5×10 -1 S / cm.