Silicone rubber oral impression material and preparation method thereof

By using microsphere catalysts prepared by paraffin and Caster catalysts, the problem of regulating working time and curing time in silicone rubber oral impression materials is solved, and rapid curing in the oral cavity and long working time is achieved, shortening the patient's waiting time .

CN118909447APending Publication Date: 2024-11-08JIAXING UNITED CHEM
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411029893.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

It is difficult to control working time and curing time at the same time in existing silicone rubber oral impression materials, resulting in the patient waiting time being too long.

Method used

Using microsphere catalysts prepared with paraffin and Caster catalysts, the Caster catalyst is released by melting paraffin in the oral cavity to promote the addition reaction between Si-H and Si-Vi, and achieve rapid curing. At the same time, when operating at room temperature The paraffin has not melted, extending working hours.

Benefits of technology

It effectively shortens the curing time of silicone rubber impression materials, shortens the waiting time for patients, and extends working time, achieving both adjustments in working time and curing time.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of oral impression materials, in particular to a silicone rubber oral impression material and a preparation method thereof. The catalyst consists of a matrix component A and a catalytic component B, the matrix component A is prepared from the following components in parts by mass: 30 to 60 parts of vinyl silicone oil, 1 to 5 parts of hydrogen-containing silicone oil, 5 to 10 parts of white carbon black, 0.01 to 0.5 part of inhibitor, 25 to 40 parts of filler and 0 to 3.5 parts of other auxiliaries; the catalytic component B comprises the following components in parts by mass: 30-60 parts of vinyl silicone oil, 0.5-5 parts of a microsphere catalyst, 5-10 parts of white carbon black, 25-40 parts of filler and 0-5 parts of other auxiliaries; the microsphere catalyst is a mixture of polyvinyl alcohol, paraffin and a Karst catalyst. According to the material disclosed by the invention, microspheres prepared from paraffin and a catalyst are used as a catalyst for triggering curing of the material, so that the curing time of the material in the oral cavity can be effectively shortened and the waiting time of a patient can be shortened under the condition that the working time is basically not influenced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of oral cavity impression materials, and in particular to a silicone rubber oral cavity impression material and a preparation method thereof. Background Art

[0002] Silicone rubber oral impression material is a highly elastic material used to make oral impressions. Oral impression is a commonly used technique in stomatology, used to make dental restorations, dentures, braces, etc. Silicone rubber oral impression material has the advantages of high elasticity, wear resistance, and not easy to deform. It can better adapt to the oral morphology and improve the accuracy and stability of the impression. At present, silicone rubber oral impression material has become one of the most commonly used impression materials in the field of stomatology.

[0003] Silicone rubber oral impression materials have relatively strict requirements on working time and curing time. Working time refers to the time from the start of mixing to the start of curing of the material, and curing time refers to the time it takes for the material to completely cure. For oral impression materials, the working time should be long enough so that the material can be fully injected into the mouth after mixing and a clear impression can be obtained. The curing time should be as short as possible so that the impression preparation can be completed as quickly as possible and the patient's waiting time can be shortened. Achieving the goal of making the working time as long as possible and the curing time as short as possible has always been the direction of everyone's efforts. However, the existing technical solutions basically increase or decrease the working time and curing time at the same time.

[0004] CN110183854A discloses a putty-type silicone rubber composition and its preparation method and application. The putty-type silicone rubber composition includes a cross-linking component and a catalytic component. The cross-linking component includes polysiloxane A, polysiloxane B, white carbon black and solid filler. The catalytic component includes polysiloxane A, polysiloxane B, white carbon black, solid filler and catalyst; the polysiloxane A is silicone oil, and the polysiloxane B is silicone rubber. The putty-type silicone rubber material of this invention is a two-component material, and the operating time and curing time that match the actual application can be obtained by changing the ratio of the cross-linking component and the catalytic component. However, in order to improve the mechanical properties of the material, its curing time is extended, and the problem of working time is not mentioned.

[0005] CN111053698A discloses an oral impression material, comprising: a catalyst component and a matrix component; by weight, the catalyst component comprises: 15-40 parts of vinyl silicone oil, 0.5-20 parts of silicone resin, 55-80 parts of reinforcing filler and 0.5-1.5 parts of platinum catalyst; by weight, the matrix component comprises: 5-25 parts of vinyl silicone oil, 0.5-20 parts of silicone resin, 55-80 parts of reinforcing filler and 5-20 parts of hydrogen-containing silicone oil. The oral impression material of the invention is composed of a catalyst and a matrix bicomponent, the matrix component comprises a base polymer and a crosslinker, the catalyst component comprises a base polymer and a catalyst, wherein vinyl silicone oil and silicone resin are used as base materials, hydrogen-containing silicone oil is used as a crosslinker, and reinforcing fillers are added to the two components at the same time, and the obtained impression material can accurately record the occlusal relationship while overcoming the disadvantages of low hardness, easy deformation and fracture. However, its working time is only about 25-30s, which is too short and requires high technical skills of the operator. Summary of the invention

[0006] Aiming at the problem that it is difficult to achieve balanced regulation of working time and curing time for oral silicone rubber impression materials, the present invention provides a silicone rubber oral impression material. The material uses microspheres prepared from paraffin and a catalyst as a catalyst for triggering the curing of the material, and can effectively shorten the curing time of the material in the oral cavity without substantially affecting the working time, thereby shortening the waiting time of patients.

[0007] To achieve the above object, the technical solution adopted by the present invention is:

[0008] A silicone rubber oral impression material, comprising a matrix component A and a catalytic component B;

[0009] The matrix component A comprises, by weight: 30-60 parts of vinyl silicone oil, 1-5 parts of hydrogenated silicone oil, 5-10 parts of white carbon black, 0.01-0.5 parts of inhibitor, 25-40 parts of filler, and 0-3.5 parts of other additives;

[0010] The catalytic component B includes, by weight: 30-60 parts of vinyl silicone oil, 0.5-5 parts of microsphere catalyst, 5-10 parts of white carbon black, 25-40 parts of filler, and 0-5 parts of other additives;

[0011] The microsphere catalyst is a mixture of polyvinyl alcohol, paraffin and Custer catalyst.

[0012] The present invention adopts paraffin wax with a temperature close to that of the oral cavity and a Custer catalyst to obtain a microsphere catalyst. When the silicone rubber impression material is used, the paraffin wax microspheres melt, thereby releasing more Custer catalyst components to trigger an addition reaction of Si-H and Si-Vi, thereby realizing rapid curing of the silicone rubber impression material. The concentration of the catalyst in the microspheres is relatively high, thereby shortening the curing time of the silicone rubber impression material. During the operation under room temperature, since the paraffin wax is not melted and less catalyst is released, a long working time can be realized during the mixing operation. Thus, the regulation of the normal temperature operation time and rapid curing in the oral cavity is realized.

[0013] The mass proportion of the Custer catalyst in the microsphere catalyst is 0-10%, not 0%; the mass proportion of polyvinyl alcohol is 1-80%, the mass proportion of paraffin is 1-20%, and the total amount is 100%. In room temperature curing addition type silicone rubber, the amount of Custer catalyst is generally 5-10ppm (effective platinum content); while the silicone rubber impression material of the present invention adds a microsphere catalyst, wherein the Custer catalyst is 20-30ppm (effective platinum content), and the amount of Custer catalyst is more than 2 times higher than that of general room temperature vulcanized silicone rubber, so the curing time of the silicone rubber impression material in the oral cavity is shortened.

[0014] Preferably, the preparation of the microsphere catalyst comprises the steps of:

[0015] Step 1, stirring and mixing the Custer catalyst and the molten paraffin, and mixing and shearing the mixed solution with the polyvinyl alcohol solution to obtain an oil-water emulsion;

[0016] Step 2, mixing the oil-water emulsion with ice-salt water to solidify to obtain paraffin microspheres, and then sieving, pre-freezing and freeze-drying to obtain the microsphere catalyst.

[0017] Preferably, in step 1, the temperature of the melted paraffin is 40-80° C., the temperature of the polyvinyl alcohol solution is 40-90° C., the solvent is water, the shearing speed is 100-800 rpm, and the shearing time is 1-60 minutes.

[0018] Preferably, in step 2, the temperature of the ice brine is -20 to 0°C, the pre-freezing temperature is -20 to 0°C, and the time is 1 to 60 minutes.

[0019] The particle size of the microsphere catalyst is 10-1000 microns, and the preferred particle size of the microsphere is 100-600 microns.

[0020] Preferably, the mass ratio of the matrix component A to the catalytic component B is 1-10:1. Preferably, the mass ratio of the matrix component A to the catalytic component B is 1-10:1.

[0021] Preferably, the vinyl content of the vinyl silicone oil is 0.15-2.0 mmol / g, the viscosity is 200-100000 CP, and the vinyl group is located at the end group or side group of the molecule; the higher the vinyl content, the faster the curing speed and the higher the hardness of the silicone rubber; the greater the viscosity of the vinyl silicone oil, the better the viscoelasticity of the silicone rubber and the slower the curing speed. The preferred vinyl silicone oil has a vinyl content of 0.5-1.5 mmol / g and a viscosity of 300-5000 CP.

[0022] Preferably, the molar content of silicon hydrogen groups in the hydrogen-containing silicone oil is 0.25-1.5%, and the viscosity is 5-1000CP; the higher the hydrogen content of the hydrogen-containing silicone oil, the faster the curing speed and the increased hardness of the silicone rubber; the greater the viscosity of the hydrogen-containing silicone oil, the better the viscoelasticity of the silicone rubber after curing and the slower the curing speed. The preferred molar content of silicon hydrogen groups in the hydrogen-containing silicone oil is 0.5-1.0%, and the viscosity is 200-600CP.

[0023] Preferably, the white carbon black is fumed white carbon black with a particle size of 20-100 nm;

[0024] Preferably, the inhibitor is one or two of tetramethyldivinyldisiloxane, tetravinyltetramethylcyclotetrasiloxane, and low-viscosity vinyl-terminated silicone oil (10-30CP).

[0025] Preferably, the filler is one or a mixture of silicon micropowder, quartz powder, aluminum hydroxide, and calcium carbonate with a particle size of 20-1000 nm;

[0026] Preferably, the other auxiliary agents include one or more of a hydrophilic modifier, a color enhancer and a flavoring essential oil, or may also include other commonly used auxiliary agents in the art.

[0027] The present invention also provides a method for preparing the silicone rubber oral impression material, comprising the steps of:

[0028] Step 1, mixing the raw materials of the matrix component A and vacuum degassing for later use; mixing the raw materials of the catalytic component B and vacuum degassing for later use;

[0029] Step 2: Mix the matrix component A and the catalytic component B in a mass ratio of 1-10:1.

[0030] Compared with the prior art, the present invention has the following beneficial effects:

[0031] (1) In the present invention, a microsphere catalyst mixed with paraffin wax having a melting point of 30-35°C and a Custer catalyst is added to the catalyst component B, which effectively prolongs the working time and shortens the curing time at the same time, thereby achieving a balanced adjustment of the working time and curing time of the oral impression material, thereby shortening the pain caused by the waiting time for patients.

[0032] (2) The oral impression material of the present invention has a wide range of raw materials, low cost, simple preparation method, mild conditions, and is conducive to industrial production and application. DETAILED DESCRIPTION

[0033] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention is further described in detail below in conjunction with embodiment. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention. Those skilled in the art can make modifications or equivalent substitutions based on the understanding of the technical scheme of the present invention without departing from the spirit and scope of the technical scheme of the present invention, and all should be included in the protection scope of the present invention.

[0034] The raw materials used in the following specific embodiments are all purchased from the market.

[0035] Example 1

[0036] Preparation of microsphere catalyst: 3g of solid paraffin wax (melting point 30℃-35℃) at room temperature was heated to 50℃ to melt, 1.5g of Custer catalyst was added, and stirred evenly to form a mixed solution; the mixed solution was slowly added to 200g of 6% polyvinyl alcohol aqueous solution at 60℃, and stirred evenly for 10 minutes under high shear (2000rpm) to form an oil-water emulsion;

[0037] The oil-water emulsion is poured into ice-salt water at a temperature of -10°C, so that the paraffin droplets in the oil-water emulsion are quickly solidified to obtain a mixture; the mixture is wet-screened, and after the wet-screening is completed, the paraffin microspheres are filtered to obtain the paraffin microspheres; the paraffin microspheres are pre-frozen at -5°C, and then freeze-dried for standby use, the average particle size of the microspheres is 500 microns, and the mass percentage of the Custer catalyst is 9%. Recorded as catalyst microspheres-1.

[0038] Example 2

[0039] Preparation of microsphere catalyst: 5g of solid paraffin wax (melting point 30℃-35℃) at room temperature was heated to 50℃ to melt, 2g of Custer catalyst was added, and stirred evenly to form a mixed solution; the mixed solution was slowly added to 200g of 1.0% polyvinyl alcohol aqueous solution at 70℃, and stirred evenly at high speed (3000rpm) to form an oil-water emulsion;

[0040] The oil-water emulsion is poured into ice-salt water at a temperature of -20°C, so that the paraffin droplets in the oil-water emulsion are quickly solidified to obtain a mixture; the mixture is wet-screened, and after the wet-screening is completed, the paraffin microspheres are filtered to obtain paraffin microspheres; the paraffin microspheres are pre-frozen at -20°C, and then freeze-dried for standby use, the microsphere particle size is 350 microns, and the mass percentage of Custer catalyst is 6.3%. It is recorded as catalyst microsphere-2.

[0041] Embodiment 3-6

[0042] The matrix component A is calculated by weight: 50 parts of vinyl silicone oil (viscosity 500CP, vinyl content 0.5mmol / g, Jiaxing United Chemical Co., Ltd.), 3 parts of hydrogen-containing silicone oil (viscosity 200CP, hydrogen content 0.5%, Jiaxing United Chemical Co., Ltd.), 8 parts of white carbon black (200 microns, Evonik Group), 0.1 parts of inhibitor tetravinyltetramethyldisiloxane, 35.5 parts of filler (3000 mesh quartz sand), and 3.0 parts of polyether surfactant (Dow Corning OFX0400).

[0043] The catalyst component B of Example 1 or 2 is calculated by weight: 45-50 parts of vinyl silicone oil (viscosity 500CP, vinyl content 0.5%, Jiaxing United Chemical Co., Ltd.), 6 parts of white carbon black (200 microns, Evonik Group), 30 parts of filler (3000 mesh quartz sand), 0.5 parts of microsphere catalyst, and 4.5 parts of polyether surfactant (Dow Corning OFX0400).

[0044] Example 3 Catalyst component B component is calculated by weight: the weight fraction of microsphere catalyst is 0.1 parts, vinyl silicone oil 45 parts (viscosity 800CP, vinyl content 0.6%, Jiaxing United Chemical Co., Ltd.), white carbon black 15 parts (200 microns, Evonik Group), filler 30 parts (3000 mesh silicon powder), polyether surfactant (Dow Corning OFX0400) 4.5 parts.

[0045] Example 4 Catalyst component B component is calculated by weight: 45-50 parts of vinyl silicone oil (viscosity 500CP, vinyl content 0.5%, Jiaxing United Chemical Co., Ltd.), 6 parts of white carbon black (200 microns, Evonik Group), 30 parts of filler (3000 mesh quartz sand), 1 part of microsphere catalyst, and 4.5 parts of polyether surfactant (Dow Corning OFX0400).

[0046] Example 5: Catalyst component B component is calculated by weight: 45-50 parts of vinyl silicone oil (viscosity 500CP, vinyl content 0.5%, Jiaxing United Chemical Co., Ltd.), 6 parts of white carbon black (200 microns, Evonik Group), 30 parts of filler (3000 mesh quartz sand), 3 parts of microsphere catalyst, and 4.5 parts of polyether surfactant (Dow Corning OFX0400).

[0047] Example 6: Vinyl silicone oil 45-50 parts (viscosity 500CP, vinyl content 0.5%, Jiaxing United Chemical Co., Ltd.), white carbon black 6 parts (200 microns, Evonik Group), filler 30 parts (3000 mesh quartz sand), microsphere catalyst 5 parts, polyether surfactant (Dow Corning OFX0400) 4.5 parts.

[0048] Example 7 Catalyst Component B component is calculated by weight: 50 parts of vinyl silicone oil (viscosity 5000CP, vinyl content 1.5mmol / g, Jiaxing United Chemical Co., Ltd.), 18 parts of white carbon black (200 microns, Evonik Group), 30 parts of filler (3000 mesh calcium carbonate), 10 parts of microsphere catalyst, and 4.5 parts of polyether surfactant (Dow Corning OFX0400).

[0049] The matrix component A and the catalyst component B are mixed evenly with a double planetary mixer and a three-roller machine, and vacuum degassing is performed. The degassing components are injected into the two-component hose by a two-component filling machine for standby use. When in use, they can be mixed evenly with a static mixing head. The matrix component A and the catalyst component B are evenly mixed in a mass ratio of 1:1.

[0050] The test was conducted in accordance with YY / T 0493 dental elastomer impression materials, and the sample was configured as Type 2. The mixed sample was injected into a stainless steel mold with a diameter of 10 mm and a thickness of 1 mm using a static mixer at room temperature (23°C ± 2°C), and after waiting for 2 minutes, it was transferred to an oven at 35°C. The Shore hardness was tested every 15 seconds to determine the approximate curing time. Then, the Shore hardness A was tested every 5 seconds starting from 30 seconds before the curing time. The curing time refers to the time from the start of polymerization until the Shore hardness A no longer changes in an oven at 35°C. The relevant test results are shown in Table 1.

[0051] Table 1 Oral impression material performance data of Examples 3-7

[0052] Indicator parameters Example 3 Example 4 Example 5 Example 6 Example 7 Working time (min:sec) 5:20 5:10 5:05 4:57 4:52 Curing time (min:sec) 5:00 4:45 3:45 3:25 3:00 Consistency(mm) 40 38 35 35 33 Detail reproduction (um) 20 20 20 20 20 Linear size change (%) 1.2 1.2 1.2 1.2 1.2 Compatibility with gypsum (um) 50 50 50 50 50 Elastic recovery rate (%) 99.5 99.5 98.5 98.5 97.5 Compression strain (%) 5.2 5.5 6.3 8.8 10.4

[0053] It can be seen from the data in Table 1 that the curing time of the impression material of Example 3 without adding a catalyst is as long as 5 minutes. As the amount of catalyst increases, the curing time is significantly shortened, while the working time is only slightly shortened and is basically unaffected, thereby effectively achieving the joint adjustment of the curing time and the working time.

Claims

1. A silicone rubber oral impression material, characterized in that: It is composed of a matrix component A and a catalytic component B; The matrix component A comprises, by weight: 30-60 parts of vinyl silicone oil, 1-5 parts of hydrogenated silicone oil, 5-10 parts of white carbon black, 0.01-0.5 parts of inhibitor, 25-40 parts of filler, and 0-3.5 parts of other additives; The catalytic component B includes, by weight: 30-60 parts of vinyl silicone oil, 0.5-5 parts of microsphere catalyst, 5-10 parts of white carbon black, 25-40 parts of filler, and 0-5 parts of other additives; The microsphere catalyst is a mixture of polyvinyl alcohol, paraffin and Custer catalyst.

2. The silicone rubber oral impression material according to claim 1, characterized in that: The mass proportion of the Custer catalyst in the microsphere catalyst is 0-10%, not 0%; the mass proportion of polyvinyl alcohol is 1-80%, the mass proportion of paraffin is 1-20%, and the total amount is 100%.

3. The silicone rubber oral impression material according to claim 1 or 2, characterized in that: The preparation of the microsphere catalyst comprises the following steps: Step 1, stirring and mixing the Custer catalyst and the molten paraffin, and mixing and shearing the mixed solution with the polyvinyl alcohol solution to obtain an oil-water emulsion; Step 2, mixing the oil-water emulsion with ice-salt water to solidify to obtain paraffin microspheres, and then sieving, prefreezing, and freeze-drying to obtain the microsphere catalyst.

4. The silicone rubber oral impression material according to claim 3, characterized in that: In step 1, the temperature of the melted paraffin is 40-80° C., the temperature of the polyvinyl alcohol solution is 40-90° C., the solvent is water, the shearing speed is 100-800 rpm, and the shearing time is 1-60 minutes.

5. The silicone rubber oral impression material according to claim 3, characterized in that: In step 2, the temperature of the ice brine is -20 to 0°C, the pre-freezing temperature is -20 to 0°C, and the time is 1 to 60 minutes; the particle size of the microsphere catalyst is 10 to 1000 microns.

6. The silicone rubber oral impression material according to claim 1, characterized in that: The mass ratio of the matrix component A to the catalytic component B is 1-10:

1.

7. The silicone rubber oral impression material according to claim 1, characterized in that: The vinyl silicone oil has a vinyl molar content of 0.15-2.0% (mol / mol), a viscosity of 200-100000 CP, and the vinyl group is located at the end group or side group of the molecule; And / or, the hydrogen-containing silicone oil has a silicon hydrogen content of 0.25-1.5% (mol / mol) and a viscosity of 5-1000 CP.

8. The silicone rubber oral impression material according to claim 1, characterized in that: The white carbon black is fumed white carbon black with a particle size of 20-200 nm; And / or, the inhibitor is tetramethyldivinyldisiloxane.

9. The silicone rubber oral impression material according to claim 1, characterized in that: The filler is one or a mixture of silicon micropowder, quartz powder, aluminum hydroxide, and calcium carbonate with a particle size of 20-1000nm; And / or, the other auxiliary agents include one or more of a hydrophilic modifier, a colorant and a flavoring essential oil.

10. The method for preparing the silicone rubber oral impression material according to any one of claims 1 to 9, characterized in that: Includes steps: Step 1, mixing the raw materials of the matrix component A and vacuum degassing for later use; mixing the raw materials of the catalytic component B and vacuum degassing for later use; Step 2: Mix the matrix component A and the catalytic component B in a mass ratio of 1-10:1.