Inorganic insulating paint for ultrathin oriented silicon steel and coating process

By using inorganic insulating coatings with phosphate and other components on the surface of ultra-thin oriented silicon steel, the adhesion and insulation problems of inorganic insulating coating on ultra-thin oriented silicon steel are solved, and high insulation resistance and Excellent magnetic performance, meet the application needs at medium and high frequencies.

CN118909468APending Publication Date: 2024-11-08HUAYU ZHIZAO (SHANGHAI) NEW MATERIALS CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411136668.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing inorganic insulating coatings have poor adhesion and insulation properties on ultra-thin oriented silicon steel surfaces, and cannot meet the insulation requirements at medium and high frequencies. Especially when there is no bottom layer, the coating is thin, and it cannot meet the ultra-thin oriented silicon steel. application requirements.

Method used

Inorganic insulating coatings using phosphate, silicon sol, magnesium oxide, chromium anhydride, nickel sulfate, borate and molybdate, to form a three-dimensional disordered amorphous network structure to adjust the insulation and adhesion of the coating , and by adjusting the specific gravity of the coating liquid and sintering temperature, the stable performance of the coating at medium and high frequencies is ensured.

Benefits of technology

A coating with excellent surface quality of the steel plate was obtained, with an insulation resistance of more than 70Ω·cm2/piece, which met the insulation requirements at medium and high frequencies, and improved magnetic performance, avoiding energy waste and reduced coating performance caused by excessive sintering temperature.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention discloses an inorganic insulating coating for ultrathin oriented silicon steel and a coating process, and belongs to the technical field of insulating coatings. The inorganic insulating coating is prepared from the following components in percentage by mass: 14 to 22 percent of phosphate, 4.5 to 9 percent of silica sol in an anhydrous manner, 0.1 to 1 percent of magnesium oxide, 1 to 5 percent of chromic anhydride, 0.2 to 1 percent of nickel sulfate, 0.5 to 3 percent of borate, 0.1 to 1 percent of molybdate and the balance of water. Coating the inorganic insulating coating liquid on the surface of ultra-thin oriented silicon steel with the thickness x of 0.03-0.10 mm obtained by cold rolling, and sintering to obtain an insulating coating; and meanwhile, the relationship between the specific gravity of the coating liquid and the thickness of the steel strip is cooperatively regulated, and the relationship among the thickness of the steel strip, the coating liquid components and the sintering temperature is cooperatively regulated. The insulation resistance of the ultra-thin oriented silicon steel is not less than 70 omega.cm < 2 > / piece, and the insulation performance of the coating at medium and high frequencies is met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of insulating coatings, and in particular relates to an inorganic insulating coating for ultra-thin oriented silicon steel and a coating process. Background Art

[0002] Ultra-thin oriented silicon steel is mainly used for high-frequency transformers, high-power electromagnetic amplifiers, pulse transformers, pulse generators, inductors, roughness and memory elements, and transformer cores working under vibration and radiation conditions. Its operating frequency is generally greater than 400 Hz. However, there is currently a lack of high-performance tension coating systems suitable for direct coating on the surface of ultra-thin oriented silicon steel, resulting in a large gap between the coating performance of domestic ultra-thin oriented silicon steel and imported products, and it cannot meet the application requirements of UHV DC projects. Especially under medium and high frequency voltages, due to the thin steel plate, in order to meet the requirements of coating and stacking coefficient, the coating cannot be too thick. In addition, because ultra-thin oriented silicon steel is different from conventional oriented silicon steel, there is no bottom layer on the surface, and only a layer of insulating coating provides insulation. If a conventional insulating coating is applied, its insulation resistance is less than 10Ω·cm 2 / piece, steel plate insulation resistance is less than 10Ω·cm 2 / piece, the steel plate is easy to break down under medium and high frequency voltages and cannot meet the requirements of UHV DC projects. The document "Preparation and Performance Evaluation of Ultra-thin Oriented Silicon Steel Coating for UHV DC Converter Valve Saturated Reactor" proposes an insulating coating for ultra-thin oriented silicon steel, which uses aluminum phosphate, nano-aluminum silicate and chromic anhydride as the main raw materials, and adds adhesion promoters, leveling agents, and high-temperature antioxidants. However, the insulation resistance of the coating can only reach 22.5Ω·cm 2 / sheet, does not meet the insulation requirements of ultra-thin oriented silicon steel under medium and high frequencies.

[0003] CN103406249A proposes a process for coating insulating paint on the surface of an ultra-thin oriented silicon steel strip. By improving the coating roller and steel strip coating method, the paint layer of the ultra-thin oriented silicon steel strip product is thin, uniform, consistent in thickness, smooth, flat and controllable.

[0004] CN111748248A proposes a chromium-free semi-organic insulating coating suitable for Bi-containing ultra-high magnetic induction oriented silicon steel without a bottom layer. It is mainly used to meet the welding performance of the Bi-containing ultra-high magnetic induction oriented silicon steel coating without a bottom layer and improve the processing performance of the oriented silicon steel coating. It is not suitable for ultra-thin oriented silicon steel strips.

[0005] CN104928567A proposes a grain-oriented silicon steel with good processing performance and a method for manufacturing the same. A semi-organic chromium-free insulating coating is coated on the surface of a steel plate after the glass film bottom layer is removed. The effective components of the chromium-free semi-organic coating are phosphate and an organic resin. After coating, the film is baked at a plate temperature of 200-450°C. A surface tension coating with high hardness and poor adhesion will not be formed on the surface of the substrate, and the steel plate has good processing performance. This method only considers the punching performance of the coating and is not suitable for extremely thin oriented silicon steel sheets.

[0006] CN113969103B proposes a semi-organic insulating coating for ultra-thin oriented silicon steel, comprising the following components: 10-25% phosphate, 1-10% epoxy-containing silane coupling agent, 0.2-2.0% organic silane, 1-10% chromic anhydride, 1.5-6% silicon dioxide particles, 0.3-5% alkali, and the balance is water; wherein the particle size of the silicon dioxide particles is 100-300nm. When the semi-organic insulating coating is applied to the surface of ultra-thin oriented silicon steel, it not only improves the adhesion of the coating to the substrate, but also ensures the insulation and heat resistance of the coating, but this method still does not meet the insulation performance of ultra-thin oriented silicon steel under medium and high frequencies.

[0007] In summary, the inorganic insulating coating used in existing oriented silicon steel is only suitable for coating on the magnesium silicate base layer. If it is directly coated on the surface of ultra-thin oriented silicon steel, the coating adhesion and insulation are poor, which cannot meet the requirements of ultra-thin oriented silicon steel. Although the adhesion of various types of semi-organic coatings used in existing non-oriented silicon steel can reach Class A, the insulation resistance is low and cannot meet the insulation requirements of ultra-thin oriented silicon steel under medium and high frequencies. The existing technologies have not considered the insulation problem of ultra-thin oriented silicon steel under medium and high frequencies when the coating is thin without a base layer, and cannot meet the application requirements of ultra-thin oriented silicon steel under medium and high frequencies. Summary of the invention

[0008] The technical problem to be solved by the present invention is to provide an insulating coating and coating process for ultra-thin oriented silicon steel in view of the deficiencies of the prior art. The steel plate coating formed by the insulating coating of the present invention has excellent surface quality, good adhesion and insulation, and an insulation resistance greater than 70Ω·cm 2 / sheet, which can meet the insulation requirements of ultra-thin oriented silicon steel under medium and high frequencies.

[0009] In order to solve the above technical problems, the present invention adopts the following technical solutions:

[0010] Provided is an inorganic insulating coating for ultra-thin oriented silicon steel. The components, calculated by mass percentage, are 14-22% phosphate, 4.5-9% anhydrous silica sol, 0.1-1% magnesium oxide, 1-5% chromic anhydride, 0.2-1% nickel sulfate, 0.5-3% borate, 0.1-1% molybdate, and the balance is water.

[0011] According to the above scheme, the borate is selected from one of the borates of Mg, Li, Na, Al, and K.

[0012] According to the above scheme, the molybdate is selected from one of ammonium molybdate, sodium molybdate and zinc molybdate.

[0013] According to the above scheme, the phosphate is selected from one of aluminum phosphate, magnesium phosphate, sodium phosphate and potassium phosphate.

[0014] A method for preparing the inorganic insulating coating for ultra-thin oriented silicon steel is provided. Magnesium oxide, chromic anhydride, nickel sulfate, borate and molybdate are added with water according to a stoichiometric ratio to form a solution. Then a phosphate solution and silica sol are added. With or without water, the inorganic insulating coating for ultra-thin oriented silicon steel is dispersed to obtain the inorganic insulating coating.

[0015] According to the above scheme, the silica sol with a solid content of 25-35% is used in the preparation process.

[0016] According to the above scheme, the solid content of the solution using phosphate in the preparation is 35-45%.

[0017] The present invention provides an inorganic insulating coating for ultra-thin oriented silicon steel, which uses phosphate as the main film-forming material of the coating to form a phosphate glass film with a three-dimensional disordered amorphous network structure on the surface of the steel plate, which is beneficial to the insulation of the coating; the HO on the surface of the colloidal SiO2 in the silica sol - The active groups such as chromium anhydride and hydroxyl groups are cross-linked with the active hydroxyl groups in the phosphate network, so that the phosphate molecules are connected through the hydrogen bonds of water molecules, the number of bridging oxygens in the amorphous network structure is increased, the degree of connection between the POP chains is enhanced, the integrity of the amorphous network connection is promoted, and the network structure strength of the film-forming material is strengthened; the chromic anhydride and magnesium oxide used can simultaneously adjust the curing film-forming speed of the film-forming material phosphate and silica sol, which is beneficial to reduce the curing temperature of the phosphate, promote the curing reaction, and make the film-forming material polyphosphate molecules cross-bonded through -O-Cr-O-bonds or -O-Mg-O-bonds to form a more complete spatial network macromolecular structure, and the simultaneous addition of the acidic oxide chromic anhydride and the alkaline oxide magnesium oxide is helpful to adjust the pH of the coating solution. In addition, magnesium oxide can react with the oxide layer in the substrate, which is beneficial to improve the adhesion of the coating; at the same time, nickel sulfate, borate and molybdate can be used to inhibit the crystallization of the film-forming material, promote the formation of an amorphous network structure, and can be based on the SO4 2- , BO4 3- 、MoO4 2 -The mutual promotion effect between them synergistically increases the tetrahedral structure in the network structure, thereby further strengthening the connectivity and tightness of the amorphous network structure and obtaining a coating with high insulation properties.

[0018] Phosphate is the main film-forming substance of the coating. As the heat treatment temperature of the coating increases, a phosphate glass film with a three-dimensional disordered network structure is formed on the surface of the steel plate, which is beneficial to the insulation of the coating. If its content is too low, it is impossible to obtain a better surface insulation resistance. The phosphate content should not be too high to prevent the free phosphoric acid in the coating from corroding the coating surface during sintering and affecting the appearance of the coating. Phosphate replaces traditional dihydrogen phosphate, has a relatively faster curing rate and a lower curing temperature, and is also conducive to the rapid film formation and curing of the coating on ultra-thin oriented silicon steel.

[0019] Chromic anhydride, as a curing agent, accelerates the dehydration process of phosphate while inhibiting its crystallization and promoting the formation of amorphous network structure, making the insulating film stronger and beneficial to the insulation of the steel strip. The chromic anhydride content should not be too high, as it will easily cause cracks to form after sintering of the coating, affecting the insulation performance of the steel strip; the content should not be too low, as it will be detrimental to the insulation of the coating on the surface of ultra-thin oriented silicon steel.

[0020] Magnesium oxide can react with the oxide layer in the substrate, which is beneficial to improve the adhesion of the coating. The magnesium oxide content should not be too high, otherwise magnesium silicate will form on the surface of the steel strip, affecting the magnetic properties of the steel strip; the magnesium oxide content should not be too low, otherwise it will be detrimental to the adhesion of the coating on the surface of ultra-thin oriented silicon steel.

[0021] Nickel sulfate, as an insulating lubricant in coatings, forms a protective film on the metal surface, which helps to improve the insulation performance of the coating at medium and high frequencies. 2- Can react with BO4 in borates and molybdates 3- 、MoO4 2 - Mutually promoting the tetrahedral structure in the amorphous network structure, strengthening the amorphous network structure of the film. The nickel sulfate content should not be too high, as it will increase nickel ions on the surface of the steel strip and affect the magnetic properties of the steel strip; the content should not be too low, as it will reduce the insulation performance of the coating at medium and high frequencies.

[0022] Borate, selected from Mg, Li, Na, Al, K and the like, can be combined with SO4 provided by nickel sulfate and molybdate by increasing the tetrahedral component [BO4] of the network structure. 2- 、MoO4 2 -The mutual promotion effect of synergistically increases the tetrahedral structure in the amorphous network structure, strengthens the network structure strength of the film-forming material, and makes the coating network structure not easy to break at medium and high frequencies, thereby improving the insulation performance of the coating at medium and high frequencies. The content should not be too high, which will affect the leveling of the coating liquid, be detrimental to the coating effect of the coating liquid on the surface of the steel strip, and easily form coating mottled defects; the content should not be too low, which will reduce the insulation performance of the coating at medium and high frequencies.

[0023] The molybdate is selected from one of ammonium molybdate, sodium molybdate and zinc molybdate, which is beneficial to promoting the film-forming reaction speed of the coating on the surface of the steel plate, and can form a passivation film of molybdenum oxide on the surface of the steel plate, thereby improving the insulation performance of the coating at medium and high frequencies. 2- SO4 can be provided by nickel sulfate and borate respectively 2- , BO4 3- The mutual promotion effect of the two ions synergistically increases the tetrahedral structure in the amorphous network structure and strengthens the amorphous network structure of the film. The content should not be too high, otherwise the molybdenum ions on the surface of the steel strip will increase, affecting the magnetic properties of the steel strip; the content should not be too low, otherwise the insulation performance of the coating at medium and high frequencies will be reduced.

[0024] A process for forming an insulating coating on ultra-thin oriented silicon steel is provided, the steps of which are:

[0025] The specific gravity of the inorganic insulating coating liquid is adjusted so that the specific gravity y of the inorganic insulating coating liquid after adjustment and the thickness x of the steel strip have the following relationship:

[0026] e x ≤y≤e 2×x Relation (1)

[0027] The specific gravity of the coating liquid affects the coating performance, as well as the insulation performance and magnetic properties. If the specific gravity of the coating liquid is too high, it is not conducive to the coating performance of the coating liquid on the surface of ultra-thin oriented silicon steel; if the specific gravity of the coating liquid is too low, it is not conducive to obtaining better coating insulation performance. Adjusting the specific gravity of the coating liquid in combination with the thickness of the steel strip is conducive to obtaining a stable coating effect of the insulating coating liquid on ultra-thin silicon steel of different thicknesses, and ultimately obtaining uniform and stable insulation performance, magnetic properties and coating adhesion;

[0028] An inorganic insulating coating liquid is applied on the surface of the ultra-thin oriented silicon steel strip with a thickness x of 0.03-0.10 mm obtained by cold rolling, and sintered; wherein:

[0029] The sintering temperature T has the following relationship with the steel plate thickness x, the anhydrous nickel sulfate percentage a%, the borate percentage b%, and the molybdate percentage c in the inorganic insulating coating:

[0030] 400+200×e x +5×(a+b+c)≤T≤400+250×e x +8×(a+b+c) Relationship (2)

[0031] In the above equations (1) and (2), y, x and T are unitless and represent specific values; y is expressed in g / cm 3 The value of x is in mm and the value of T is in °C.

[0032] In the inorganic insulating coating, on an anhydrous basis, a% represents the percentage of nickel sulfate, b% represents the percentage of borate, and c% represents the percentage of molybdate. At the same time, a, b and c are specific values ​​before % (for example, if the percentage of nickel sulfate is 0.5%, then a represents 0.5).

[0033] During the sintering process, the nickel sulfate, borate, and molybdate in the insulating coating liquid will inhibit the crystallization of the film-forming material and promote the formation of an amorphous network structure. 2- , BO4 3- 、MoO4 2- The mutual promotion between them synergistically increases the tetrahedral structure in the network structure, strengthens the connectivity and tightness of the network structure, and affects the amorphous network structure of the film-forming material, and then affects the insulation of the coating. The content of nickel sulfate, borate, and molybdate in the coating liquid affects the selection of sintering temperature; in addition, the thickness of the steel plate affects the heat transfer rate. For example, when the thickness is ultra-thin (less than 0.10mm), the heat transfer of the steel strip along the thickness direction is faster. At the same time, the sintering temperature used for sintering after applying the insulating coating liquid is regulated by combining the content of nickel sulfate, borate, and molybdate and the thickness of the steel plate. On the one hand, it ensures the curing effect of the coating, and obtains ultra-thin oriented silicon steel with high insulation and excellent magnetic properties; on the other hand, it can effectively control and avoid excessive sintering temperature and reduce energy waste. The sintering temperature should not be too high, which will cause the coating to be overburned, which will easily reduce the insulation and adhesion of the coating, and reduce the magnetism of the steel strip; if the sintering temperature is too low, the coating is not completely cured, and the insulation of the coating is also reduced. And because the annealing process is carried out in air, too high a temperature may cause oxidation of the steel strip, affecting the surface quality and magnetic properties of the steel strip.

[0034] According to the above scheme, the thickness of the insulating coating is 0.5-1.5 μm. Appropriate coating thickness is helpful to obtain an insulating coating with better insulating and magnetic properties.

[0035] According to the above scheme, the suitable sintering time of the obtained insulating coating is preferably 100-300s.

[0036] According to the above scheme, the ultra-thin oriented silicon steel strip is made of bottom-free oriented silicon steel with a thickness of 0.20-0.30 mm as raw material, and is prepared by cold rolling to a steel strip thickness x of 0.03-0.10 mm, alkali washing, and annealing.

[0037] Preferably, the cold rolling is performed using a 20-roll rolling mill, and the 0.20-0.30 mm bottom-free oriented silicon steel is rolled to 0.03-0.10 mm through 3-5 rolling passes.

[0038] Preferably, after cold rolling, the obtained cold-rolled strip is sent to an alkali washing tank for alkali washing to remove oil stains on the surface of the cold-rolled strip, and then washed with water, and quickly dried with hot air at 40-50°C.

[0039] Preferably, annealing is performed after cold rolling and alkali washing, the annealing temperature is 800-950° C., the annealing time is 1-5 min, and the atmosphere is a nitrogen-hydrogen mixed gas.

[0040] The present invention also provides an ultra-thin oriented silicon steel with an insulating coating formed by the above process.

[0041] According to the above scheme, the interlayer resistance of the ultra-thin oriented silicon steel is greater than 70Ω·cm 2 / piece.

[0042] The beneficial effects of the present invention are:

[0043] 1. The present invention provides an inorganic insulating coating for ultra-thin oriented silicon steel, which mainly uses phosphate and silica sol as film-forming materials, and is combined with chromic anhydride and magnesium oxide to simultaneously adjust the curing film-forming speed of the film-forming materials phosphate and silica sol, and then cooperates with nickel sulfate, borate and molybdate to strengthen the network structure material of the film-forming material, thereby improving the bond strength of the network structure of the film-forming material. When used for coating ultra-thin oriented silicon steel, the surface quality of the steel plate is excellent, and a coating with high insulation and magnetic properties can be obtained.

[0044] 2. The present invention provides a coating process for an ultra-thin oriented silicon steel insulating coating, which is conducive to stabilizing the coating effect of the insulating coating on ultra-thin silicon steels of different thicknesses by coordinating the specific gravity of the coating and the thickness of the steel strip, and obtaining uniform and stable insulation performance and coating adhesion after sintering; by coordinating the thickness of the steel strip, the coating composition and the sintering temperature, the curing effect of the coating under different steel strip thicknesses and different coating composition is ensured, thereby obtaining a coating with high insulation and ultra-thin oriented silicon steel with excellent magnetic properties, and can effectively avoid excessive sintering temperature and reduce energy waste. The insulation resistance of the ultra-thin oriented silicon steel obtained by the preparation method of the present invention is not less than 70Ω·cm 2 / pieces, meeting the insulation performance of the coating at medium and high frequencies. DETAILED DESCRIPTION

[0045] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0046] The embodiment of the present invention prepares ultra-thin oriented silicon steel according to the following steps:

[0047] The raw material of 0.20-0.30mm thick bottom-free oriented silicon steel is used as raw material, and a 20-roll rolling mill is used to roll the raw material of 0.20-0.30mm bottom-free oriented silicon steel to 0.03-0.10mm through 3-5 passes of rolling. The cold-rolled strip is sent to an alkali washing tank to remove the oil stains on the surface of the cold-rolled strip with 70-90% sodium hydroxide, and then washed with water, and the strip is quickly dried with hot air at 40-50°C. Then, recrystallization continuous annealing is carried out, the annealing temperature is 890°C, the annealing time is 3 minutes, and the atmosphere is a nitrogen-hydrogen mixed gas, so that ultra-thin oriented silicon steel with a thickness of 0.03-0.10mm is obtained.

[0048] The embodiment of the present invention provides an inorganic insulating coating for ultra-thin oriented silicon steel. The components, by mass percentage, are phosphate: 14-22%, silica sol (anhydrous): 4.5-9%, magnesium oxide: 0.1-1%, chromic anhydride: 1-5%, nickel sulfate: 0.2-1%, borate: 0.5-3%, molybdate: 0.1-1%, and the balance is water.

[0049] An embodiment of the present invention also provides a method for preparing the above-mentioned inorganic insulating coating for ultra-thin oriented silicon steel, comprising adding water to magnesium oxide, chromic anhydride, nickel sulfate, borate, and molybdate in a stoichiometric ratio to form a solution, and then adding a phosphate solution and silica sol, with or without adding water, to disperse and obtain the inorganic insulating coating for ultra-thin oriented silicon steel.

[0050] In some specific embodiments, silica sol with a solid content of 25-35% is used in the formulation, and the solvent is water.

[0051] In some specific embodiments, the solid content of the phosphate solution used in the formulation is 35-45%.

[0052] The embodiment of the present invention further provides a process for forming an insulating coating on ultra-thin oriented silicon steel, the steps of which are:

[0053] The specific gravity of the inorganic insulating coating liquid is adjusted so that the specific gravity y of the inorganic insulating coating liquid after adjustment and the thickness x of the steel strip have the following relationship:

[0054] e x ≤y≤e 2×x Relation (1)

[0055] An inorganic insulating coating liquid is applied on the surface of the ultra-thin oriented silicon steel strip with a thickness x of 0.03-0.10 mm obtained by cold rolling, and sintered; wherein:

[0056] The sintering temperature T has the following relationship with the steel plate thickness x, the anhydrous nickel sulfate content a%, the borate content b%, and the molybdate content c% in the inorganic insulating coating solution:

[0057] 400+200×e x+5×(a+b+c)≤T≤400+250×e x +8×(a+b+c) Relationship (2)

[0058] In the above equations (1) and (2), y, x and T are unitless and represent specific values; y is expressed in g / cm 3 The values ​​of x are in mm and T is in °C. In inorganic insulating coatings, on an anhydrous basis, a% represents the percentage of nickel sulfate, b% represents the percentage of borate, and c% represents the percentage of molybdate. Meanwhile, a, b and c are the specific values ​​before % (for example, if the percentage of nickel sulfate is 0.5%, a represents 0.5).

[0059] In some specific embodiments, the thickness of the insulating coating is 0.5-1.5 μm.

[0060] In some specific embodiments, the sintering time of the obtained insulating coating is 100-300 seconds.

[0061] The following are specific embodiments.

[0062] Example 1

[0063] An inorganic insulating coating for improving the insulation performance of ultra-thin oriented silicon steel at medium and high frequencies, wherein the components are calculated by weight percentage, aluminum phosphate: 14%, silica sol in anhydrous form: 4.5%, magnesium oxide: 0.1%, chromic anhydride: 1%, nickel sulfate: 0.2%, sodium borate: 0.5%, sodium molybdate: 0.1%, and the balance is deionized water, see Table 1. The solid content of the silica sol is 30±3wt%.

[0064] The specific gravity of the inorganic insulating coating liquid is adjusted to 1.06 g / cm 3 The coating was applied on 0.03 mm ultra-thin oriented silicon steel, sintered at 635 °C for 100 s, and the coating thickness was 0.5 μm. The process was shown in Table 2. The properties of the obtained steel plate are shown in Table 3.

[0065] Embodiment 2-8

[0066] Specifically refer to Example 1, wherein the composition and proportion of the inorganic insulating coating are shown in Table 1, the sintering process parameters are shown in Table 2, and the properties of the obtained steel plate are shown in Table 3.

[0067] Comparative Example 1-2

[0068] Specifically refer to Example 1, wherein the composition and proportion of the inorganic insulating coating are shown in Table 1, the sintering process parameters are shown in Table 2, and the properties of the obtained steel plate are shown in Table 3.

[0069] Table 1. Inorganic insulating coating composition and ratio in the examples and comparative examples

[0070]

[0071] In Table 1, the phosphate is added in the form of a phosphate solution, the solid content of which is 40±2%, and the solid content of the silica sol is 30±3%.

[0072] Table 2. Sintering process of insulating coating in Examples and Comparative Examples

[0073]

[0074] Table 3. Properties of steel plates obtained in Examples and Comparative Examples

[0075]

[0076] It can be seen from Table 1, Table 2 and Table 3 that in Examples 1 to 8, the insulating coating prepared according to the present invention is coated on the ultra-thin oriented silicon steel, and after sintering and annealing according to the process in Table 2, the steel plate has excellent surface quality, excellent magnetic properties, and the coating adhesion is Class A. The interlayer resistance is generally greater than 70Ω·cm 2 / sheet, meeting the insulation requirements of ultra-thin oriented silicon steel under medium and high frequencies.

[0077] In Comparative Example 1, nickel sulfate and molybdate are not added, the relationship between the specific gravity of the coating and the thickness of the steel plate does not satisfy the formula (1) proposed in the present invention, the relationship between the coating sintering temperature and the thickness of the steel plate does not satisfy the formula (2) proposed in the present invention, the specific gravity of the coating is too large, and the sintering temperature is too high, resulting in coating mottled defects on the surface, the coating adhesion is reduced to Class B, and the iron loss of the steel strip is increased, and the magnetic properties are reduced. The insulation resistance of the coating is reduced to 5.3Ω·cm 2 / sheet, does not meet the insulation requirements of ultra-thin oriented silicon steel under medium and high frequencies.

[0078] In comparative example 2, the contents of nickel sulfate, borate and molybdate do not meet the requirements of the present invention, the relationship between the specific gravity of the coating and the thickness of the steel plate does not meet the formula (1) proposed by the present invention, the specific gravity of the coating is too low, the relationship between the sintering temperature of the coating and the thickness of the steel plate does not meet the formula (2) proposed by the present invention, the sintering temperature of the coating is too high, the coating is over-burned, and finally the coating mottled appears on the surface of the ultra-thin oriented silicon steel, the adhesion is reduced to Class C, the iron loss of the steel strip is increased, and the magnetic properties are reduced. The insulation resistance of the steel plate is reduced to 4.5Ω·cm 2 / sheet, does not meet the insulation requirements of ultra-thin oriented silicon steel under medium and high frequencies.

[0079] It should be understood that those skilled in the art can make improvements or changes based on the above description, and all these improvements and changes should fall within the scope of protection of the appended claims of the present invention.

Claims

1. An inorganic insulating coating for ultra-thin oriented silicon steel, It is characterized in that The components are calculated by weight percentage: phosphate: 14-22%, silica sol: 4.5-9% on anhydrous basis, magnesium oxide: 0.1-1%, chromic anhydride: 1-5%, nickel sulfate: 0.2-1%, borate: 0.5-3%, molybdate: 0.1-1%, and the balance is water.

2. The inorganic insulating coating according to claim 1, It is characterized in that The borate is selected from one of Mg, Li, Na, Al, and K borates; the molybdate is selected from one of ammonium molybdate, sodium molybdate, and zinc molybdate; and the phosphate is selected from one of aluminum phosphate, magnesium phosphate, sodium phosphate, and potassium phosphate.

3. The inorganic insulating coating according to claim 1, It is characterized in that The solid content of the silica sol is 25-35%.

4. A method for preparing the inorganic insulating coating for ultra-thin oriented silicon steel according to claim 1, It is characterized in that Magnesium oxide, chromic anhydride, nickel sulfate, borate and molybdate are added with water according to the stoichiometric ratio to prepare a solution, and then a phosphate solution and silica sol are added, and with or without water, the inorganic insulating coating for ultra-thin oriented silicon steel is dispersed.

5. A process for forming an insulating coating on ultra-thin oriented silicon steel. It is characterized in that The steps are: The specific gravity of the inorganic insulating coating liquid according to claim 1 is regulated so that the specific gravity y of the inorganic insulating coating liquid after regulation and the thickness x of the steel strip have the following relationship: e x ≤y≤e 2×x Relation (1) An inorganic insulating coating liquid is applied on the surface of the ultra-thin oriented silicon steel strip with a thickness x of 0.03-0.10 mm obtained by cold rolling, and sintered; wherein: The sintering temperature T has the following relationship with the steel plate thickness x, the anhydrous nickel sulfate percentage a%, the borate percentage b%, and the molybdate percentage c in the inorganic insulating coating: 400+200×e x +5×(a+b+c)≤T≤400+250×e x +8×(a+b+c) Relationship (2) In the above equations (1) and (2), y, x and T are unitless and represent specific values; y is expressed in g / cm 3 The value of x is in mm and the value of T is in °C.

6. The process according to claim 5, It is characterized in that The obtained insulating coating has a thickness of 0.5-1.5 μm.

7. The process according to claim 5, It is characterized in that The sintering time of the obtained insulating coating is 100-300s.

8. The process according to claim 5, It is characterized in that The ultra-thin oriented silicon steel strip is made of bottom-free oriented silicon steel with a thickness of 0.20-0.30 mm as raw material, and is prepared by cold rolling to a steel strip thickness x of 0.03-0.10 mm, alkali washing, and annealing.

9. An ultra-thin oriented silicon steel with an insulating coating formed by the process of claim 5.

10. The ultra-thin oriented silicon steel with insulating coating according to claim 9, It is characterized in that The interlayer resistance of the ultra-thin oriented silicon steel is greater than 70Ω·cm 2 / piece.

Citation Information

Patent Citations

  • Technology method for coating insulating paint on surface of extremely thin orientated silicon steel strip

    CN103406249A

  • Grain-oriented silicon steel with good machining performance and production method thereof

    CN104928567A

  • C chromium-free semi-organic insulating coating suitable for Bi-containing ultrahigh magnetic induction oriented silicon steel without bottom layer

    CN111748248A

  • A semi-organic insulating coating for ultra-thin oriented silicon steel

    CN113969103B