Non-intumescent fireproof coating as well as preparation method and application thereof
By optimizing the formulation and process of non-expanded fire-retardant coatings, a coating with multiple sizes of holes is formed, which solves the problem of the fire resistance of the FRP reinforcement system at high temperatures, significantly improves the fire resistance, extends the fire resistance limit of the structure, and ensures that Fire safety.
Patent Information
- Application Number
- CN202411148586.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-08-21
AI Technical Summary
The performance of the binder of the existing fiber reinforced composite material (FRP) deteriorates at high temperatures, resulting in poor fire resistance of FRP reinforced concrete components, which is difficult to meet fire safety requirements. The existing non-expanded fire-retardant coatings have poor protection effect on FRP.
Using a non-expanded fire-resistant coating, the raw materials of which include metakaolin, fly ash, expanded vermiculite, vitrified microbeads, aluminum hydroxide, magnesium hydroxide, glass fiber and additives, through the optimization of the formulation and process, the Coatings with multiple sizes of pores, methods to improve thermal insulation performance and protect FRP reinforcement systems.
It effectively improves the fire resistance performance of fiber reinforced composite materials, delays the damage time of the FRP reinforcement system in fire, provides more sufficient escape and rescue time, and reduces the harm and losses caused by the fire.
Smart Images

Figure BDA0005002932700000081 
Figure BDA0005002932700000101 
Figure HDA0005002932710000011
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of fireproof materials, and in particular relates to a non-expansion fireproof coating and a preparation method and application thereof. Background Art
[0002] In recent years, fiber reinforced plastics (FRP) have become a very popular reinforcement material due to their advantages such as light weight, high strength, good durability and convenient construction. Although the FRP material reinforcement method has many advantages, this method also has a disadvantage that cannot be ignored, that is, the high temperature resistance is extremely poor. The adhesives used to paste FRP materials in the construction field are mostly epoxy resin polymers. Some studies have shown that the various properties of such adhesives will deteriorate significantly at around 75°C, resulting in poor fire resistance of FRP reinforced concrete components without fire protection in fires, making it difficult to meet the corresponding fire resistance requirements, which brings great hidden dangers to the fire safety of such structures. At present, the fire protection of FRP reinforced structures mainly adopts fireproof boards or fireproof coatings to ensure that the reinforced structures can meet the requirements of relevant specifications. Among them, non-expanding fireproof coatings are the most widely used. Although the fire resistance limit of the structure under the protection of fireproof coatings can meet the requirements of the specifications, its protection effect on FRP adhesives is not ideal. At high temperatures, the temperature at the FRP exceeds 100°C in a very short time. At this temperature, the mechanical properties of epoxy resins are significantly reduced and the function of transmitting force is lost. This shows that fire retardant coatings actually protect reinforced concrete and slow down the degradation of reinforced concrete material performance, thereby extending the fire resistance limit of the structure, but this is not suitable for FRP reinforcement systems. At present, FRP materials have been widely used in the field of building reinforcement, but the research on fire retardant coatings that match them is obviously lagging behind. Summary of the invention
[0003] In view of this, the object of the present invention is to provide a non-expanding fire retardant coating and a preparation method and application thereof. The coating formed by the non-expanding fire retardant coating provided by the present invention has excellent thermal insulation properties and can be used as a fire retardant coating for fiber reinforced composite materials (FRP).
[0004] In order to achieve the above object, the present invention provides the following technical solutions:
[0005] The present invention provides a non-expansion fire retardant coating, the preparation raw materials of which include a binder, a heat-insulating filler, a flame retardant, fibers, an additive and water:
[0006] The binder comprises metakaolin, fly ash and an activator;
[0007] The heat-insulating filler includes expanded vermiculite, vitrified microspheres, sepiolite and hollow glass microspheres;
[0008] The flame retardant includes aluminum hydroxide and magnesium hydroxide;
[0009] The fibers include glass fibers and / or carbon fibers;
[0010] The auxiliary agents include a foaming agent, a thickener, a foam stabilizer and acrylic emulsion.
[0011] Preferably, the hollow glass microspheres include two types of hollow glass microspheres with a particle size of D50 = 65 μm and a particle size of D50 = 40 μm; the volume ratio of the two types of hollow glass microspheres with a particle size of D50 = 65 μm and a particle size of D50 = 40 μm is 7:3.
[0012] Preferably, the mass of the flame retardant is 2.3-8.2% of the mass of the non-expanding fire retardant coating; and the mass ratio of the aluminum hydroxide to the magnesium hydroxide is 1.5-2.5:1.
[0013] Preferably, the blowing agent comprises sodium α-olefin sulfonate.
[0014] Preferably, the foam stabilizer comprises calcium stearate and / or a commercial powdered foam stabilizer.
[0015] Preferably, the thickener comprises sodium hydroxymethylcellulose and / or cellulose ether.
[0016] Preferably, the mass ratio of the metakaolin to fly ash is 5-7:3-5.
[0017] The present invention also provides a method for preparing the non-expanding fire retardant coating according to the above technical solution, comprising the following steps:
[0018] A binder other than the activator, a heat-insulating filler other than the hollow glass microspheres, and a flame retardant are first mixed to obtain a base material;
[0019] The base material, foaming agent, thickener and foam stabilizer are mixed for the second time to obtain a dry material;
[0020] The dry material and hollow glass microspheres are mixed for a third time, and then an activator, acrylic emulsion and water are added for a fourth mixing to obtain a mixture;
[0021] The mixed material and the fibers are mixed and dispersed to obtain a non-expanding fire retardant coating.
[0022] The present invention also provides the use of the non-expanding fire retardant coating described in the above technical solution or the non-expanding fire retardant coating prepared by the preparation method described in the above technical solution in fire prevention of fiber reinforced composite materials.
[0023] The present invention also provides a method for preparing a non-expansion fire retardant coating, comprising the following steps: coating the non-expansion fire retardant coating on the surface of the fiber-reinforced composite material, and performing curing to obtain the non-expansion fire retardant coating;
[0024] The non-expanding fire retardant coating is the non-expanding fire retardant coating described in the above technical solution or the non-expanding fire retardant coating prepared by the preparation method described in the above technical solution.
[0025] The invention provides a non-expanding fireproof coating, and the raw materials for preparing the coating include a binder, a heat-insulating filler, a flame retardant, fibers, an auxiliary agent and water: the binder includes metakaolin, fly ash and an activator; the heat-insulating filler includes expanded vermiculite, vitrified microspheres, sepiolite and hollow glass microspheres; the flame retardant includes aluminum hydroxide and magnesium hydroxide; the fibers include glass fibers and / or carbon fibers; and the auxiliary agent includes a foaming agent, a thickener, a foam stabilizer and acrylic emulsion.
[0026] The coating formed by the non-expandable fire-retardant coating provided by the present invention contains pores of three sizes, which is conducive to the improvement of thermal insulation performance. First, the geopolymer gelling material generated by the reaction of metakaolin, fly ash and an activator itself has a large number of nano-scale gel pores, and adsorbs a certain amount of free water, and evaporates and absorbs heat at high temperature, which is conducive to thermal insulation. Hollow glass microspheres are added to the coating, and the thermal conductivity coefficient is low. The addition of hollow glass microspheres can introduce micron-level pores in the coating to improve the thermal insulation performance of the coating, and can also improve the fluidity of the coating. A foaming agent is added to the coating, so that micron or even millimeter-level pores are formed in the coating. The foaming agent can not only introduce pores to improve the thermal insulation performance, but also reduce the amount of water used in the preparation. The flame retardant decomposes under heat, can absorb heat, reduce the temperature rise trend of the building components, and is also conducive to improving the thermal insulation performance of the coating, so that it can better protect the FRP reinforcement system, which is conducive to the FRP reinforcement system to continue to play a reinforcement role under fire, and will not be destroyed in a short time after the fire occurs. This provides more sufficient time for people to escape and rescue under fire, and can effectively reduce the hazards and losses caused by fire. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 This is the compression test diagram;
[0028] Figure 2 This is the bending test diagram;
[0029] Figure 3 This is the bonding strength direct pull test diagram;
[0030] Figure 4 This is a water resistance test diagram;
[0031] Figure 5 This is a schematic diagram of the fire resistance test;
[0032] Figure 6 This is a diagram of the fire resistance performance of the non-expanding fire retardant coating prepared in Example 1. DETAILED DESCRIPTION
[0033] The present invention provides a non-expansion fire retardant coating, the preparation raw materials of which include a binder, a heat-insulating filler, a flame retardant, fibers, an additive and water:
[0034] The binder comprises metakaolin, fly ash and an activator;
[0035] The heat-insulating filler includes expanded vermiculite, vitrified microspheres, sepiolite and hollow glass microspheres;
[0036] The flame retardant includes aluminum hydroxide and magnesium hydroxide;
[0037] The fibers include glass fibers and / or carbon fibers;
[0038] The auxiliary agents include a foaming agent, a thickener, a foam stabilizer and acrylic emulsion.
[0039] Unless otherwise specified, the present invention has no special requirements on the sources of the raw materials used in the preparation, and commercially available products known to those skilled in the art can be used.
[0040] The raw materials for preparing the non-expanding fire retardant coating provided by the present invention include a binder. In the present invention, the binder includes metakaolin, fly ash and an activator.
[0041] In the present invention, the particle size of the metakaolin is preferably 0.4-200 μm, more preferably D50 particle size = 9.1 μm; the particle size of the fly ash is preferably 0.32-317 μm, more preferably D50 particle size = 5.2 μm; the activator is preferably a water glass activator; the water glass activator is preferably a mixed solution of sodium silicate and sodium hydroxide; the modulus of the activator is preferably 1.2-2M, more preferably 1.3-1.6M.
[0042] In the present invention, the mass ratio of the metakaolin and fly ash is preferably 5-7:3-5, more preferably 7:3; the mass ratio of the metakaolin and the activator is preferably 70:123-134, more preferably 70:134; the mass of the binder is preferably 53.1-65.4% of the mass of the non-expanding fire retardant coating, more preferably 53.6-55%.
[0043] In the present invention, the binder preferably also includes: redispersible latex powder and / or polyvinyl alcohol powder, more preferably redispersible latex powder and polyvinyl alcohol powder; the particle size of the redispersible latex powder is preferably 1-7 μm, more preferably 3-5 μm; the particle size of the polyvinyl alcohol powder is preferably 120 mesh; the number average molecular weight of the polyvinyl alcohol powder is preferably 72600-81400, more preferably 80000; the mass ratio of the kaolin and the redispersible latex powder is preferably 70:0-5, more preferably 70:2-5; the mass ratio of the kaolin and the polyvinyl alcohol powder is preferably 70:0-1.5, more preferably 70:0.5-1.5.
[0044] In the present invention, the geopolymer gelling material generated by the reaction of metakaolin, fly ash and activator has a large number of nano-scale gel pores and adsorbs a certain amount of free water, which absorbs heat by evaporation at high temperature and is beneficial to heat insulation. The redispersible latex powder and polyethylene can improve the bonding strength of the coating.
[0045] The raw materials for preparing the non-expanding fireproof coating provided by the present invention include heat-insulating fillers. In the present invention, the heat-insulating fillers include expanded vermiculite, vitrified microspheres, sepiolite and hollow glass microspheres.
[0046] In the present invention, the particle size of the expanded vermiculite is preferably 68-564 μm, more preferably D50 particle size = 226.6 μm; the particle size of the vitrified microspheres is preferably 1-2 mm; the particle size of the sepiolite is preferably 300-400 μm, more preferably 350-400 μm; the hollow glass microspheres preferably include two hollow glass microspheres with D50 particle size = 65 μm and D50 particle size = 40 μm; the volume ratio of the two hollow glass microspheres with D50 particle size = 65 μm and D50 particle size = 40 μm is preferably 7:3; the wall thickness of the hollow glass microspheres is preferably 1-3 μm, more preferably 2 μm; the true density of the hollow glass microspheres with D50 particle size = 40 μm is preferably 0.59-0.63 g / cm 3 , more preferably 0.6 g / cm 3 The bulk density is preferably 0.33 to 0.36 g / cm 3 , more preferably 0.35 g / cm 3 The actual density of hollow glass microspheres with a particle size of D50 = 65 μm is preferably 0.19 to 0.23 g / cm 3 , more preferably 0.2 g / cm 3 The bulk density is preferably 0.09 to 0.12 g / cm 3 , more preferably 0.1 g / cm 3 .
[0047] In the present invention, the mass ratio of the expanded vermiculite to the hollow glass microspheres is preferably 43.8:17.4-21.6, more preferably 43.8:17.4; the mass ratio of the vitrified microspheres to the hollow glass microspheres is preferably 14.6:21.6 or 21.9:17.4, more preferably 21.9:17.4; the mass ratio of the sepiolite to the hollow glass microspheres is preferably 15.4:17.4-21.6, more preferably 15.4:17.4; the mass ratio of the thermal insulation filler is preferably 13.4-22.8% of the mass of the non-expanding fire retardant coating, more preferably 15-22.5%.
[0048] In the present invention, firstly, the density of expanded vermiculite and vitrified microspheres is low, which can effectively reduce the density of fire retardant coatings. In addition, the expanded vermiculite has a cavity structure inside and a layered structure, and has good thermal insulation performance. Vitrified microspheres also have a porous microstructure, which can also improve the thermal insulation performance of fire retardant coatings. The pores of both are micron-level pores. Sepiolite contains a large amount of fiber-like hydrous magnesium silicate with a large aspect ratio, which absorbs heat in combination with water evaporation at high temperature, which is conducive to delaying the conduction of heat; in addition, sepiolite also has a certain toughening effect.
[0049] In the present invention, the hollow glass microspheres have a low thermal conductivity. The addition of the hollow glass microspheres can introduce micrometer-sized pores into the coating, thereby improving the thermal insulation performance of the coating, and can also improve the working performance of the coating.
[0050] The raw materials for preparing the non-expanding fire-retardant coating provided by the present invention include a flame retardant. In the present invention, the flame retardant includes aluminum hydroxide and magnesium hydroxide; the mass of the flame retardant is preferably 2.3-8.2% of the mass of the non-expanding fire-retardant coating, more preferably 3-4.5%; the mass ratio of the aluminum hydroxide to the magnesium hydroxide is preferably 1.5-2.5:1, more preferably 2.08:1.
[0051] In the present invention, the flame retardant decomposes under heat and can absorb heat, thereby reducing the temperature rise trend of the building component and also being beneficial to improving the thermal insulation performance of the coating.
[0052] The raw materials for preparing the non-expanding fire retardant coating provided by the present invention include fibers. In the present invention, the fibers preferably include glass fibers and / or carbon fibers, more preferably glass fibers; the length of the fibers is preferably 6 to 12 mm, more preferably 6 mm; the diameter of the fibers is preferably 5 to 20 μm, more preferably 8 to 15 μm; the mass of the fibers is preferably 0.22 to 0.82% of the mass of the non-expanding fire retardant coating, more preferably 0.25 to 0.45%. The role of the fibers in the present invention is to increase the toughness of the coating and reduce the risk of cracking.
[0053] The raw materials for preparing the non-expanding fire-retardant coating provided by the present invention include auxiliary agents. In the present invention, the auxiliary agents include foaming agents, thickeners, foam stabilizers and acrylic emulsions.
[0054] In the present invention, the foaming agent preferably includes sodium α-olefin sulfonate; the foam stabilizer preferably includes calcium stearate and / or a commercial powder foam stabilizer, more preferably calcium stearate and a commercial powder foam stabilizer; the mass ratio of calcium stearate to commercial powder foam stabilizer is preferably 1:2-0.5, more preferably 1:1; the thickener preferably includes sodium hydroxymethyl cellulose and / or cellulose ether, more preferably sodium hydroxymethyl cellulose and cellulose ether; the mass ratio of sodium hydroxymethyl cellulose to cellulose ether is preferably 1:2-0.5, more preferably 1:1. In the present invention, the manufacturer of the commercial powder foam stabilizer is Luoyang Tongrun Nanotechnology Co., Ltd., model: lightweight partition board foam stabilizer.
[0055] In the present invention, the foam stabilizer will be dispersed at the gas-liquid interface of the bubbles, which is beneficial to the stability of the bubbles and prevents the bubbles from bursting. In addition, the foam stabilizer can also optimize the bubble structure. The thickener has the function of increasing the viscosity of the coating, refining the pores formed by the foaming agent, making the coating easy to apply, and improving the anti-sagging and dripping capabilities.
[0056] In the present invention, the mass ratio of the foaming agent to the thickener is preferably 0.1-0.3:0.07, more preferably 0.2:0.07; the mass ratio of the foaming agent to the foam stabilizer is preferably 0.1-0.3:0.5, more preferably 0.2:0.5; the mass ratio of the foaming agent to the acrylic emulsion is preferably 0.1-0.3:1, more preferably 0.2:1; the mass of the auxiliary agent is preferably 0.37-0.87% of the mass of the non-intumescent fire retardant coating, more preferably 0.4-0.6%.
[0057] In the present invention, the foaming agent can form micrometer-level or even millimeter-level pores in the coating. The foaming agent can not only introduce pores to improve the thermal insulation performance, but also reduce the amount of water used in the preparation.
[0058] The raw material for preparing the non-expandable fire retardant coating provided by the present invention includes water. In the present invention, the mass of the water is preferably 14.3-22.1% of the mass of the non-expandable fire retardant coating, and more preferably 15-18.1%.
[0059] The non-expandable fireproof coating provided by the present invention is based on geopolymer and various lightweight heat-insulating fillers and flame retardants are dispersed therein, and the bonding strength is improved by adding redispersible latex powder and polyethylene. In addition, various additives are added to improve the working performance and durability.
[0060] The present invention optimizes the dosage of various preparation raw materials in the non-expanding fire retardant coating, so that the prepared coating contains pores of various sizes, which is beneficial to the improvement of heat insulation performance.
[0061] The present invention also provides a method for preparing the non-expanding fire retardant coating according to the above technical solution, comprising the following steps:
[0062] A binder other than the activator, a heat-insulating filler other than the hollow glass microspheres, and a flame retardant are first mixed to obtain a base material;
[0063] The base material, foaming agent, thickener and foam stabilizer are mixed for the second time to obtain a dry material;
[0064] The dry material and hollow glass microspheres are mixed for a third time, and then an activator, acrylic emulsion and water are added for a fourth mixing to obtain a mixture;
[0065] The mixed material and the fibers are mixed and dispersed to obtain a non-expanding fire retardant coating.
[0066] In the present invention, the first mixing is preferably performed under low-speed stirring; the rate of the low-speed stirring is preferably 130-150 rpm, more preferably 140 rpm; the time of the first mixing is preferably 3-5 min, more preferably 3 min.
[0067] In the present invention, the second mixing is preferably carried out under low-speed stirring; the low-speed stirring rate is preferably 130-150 rpm, more preferably 140 rpm; the second mixing time is preferably 1-3 min, more preferably 1 min; the equipment used for the second mixing is preferably a stirring pot. During the second mixing process, the present invention preferably uses a cover plate to cover the top of the stirring pot to prevent the added additive from splashing out.
[0068] In the present invention, the third mixing is preferably carried out by manual stirring first, and then by low-speed stirring; the rate of the low-speed stirring is preferably 130-150rpm, more preferably 140rpm; the time of the low-speed stirring is preferably 1min; the equipment used for the third mixing is preferably a stirring pot. During the third mixing process, the present invention preferably uses a cover plate to cover the top of the stirring pot. Since the density of the hollow glass microspheres is extremely low, they are first dispersed in the dry material by manual stirring, and then stirred at a low speed.
[0069] In the present invention, the acrylic emulsion and water are preferably used in the form of a mixture of acrylic emulsion and water; the preparation method of the mixture of acrylic emulsion and water is preferably to mix and stir the acrylic emulsion and water uniformly; the stirring rate is preferably 30 to 50 rpm, more preferably 30 rpm.
[0070] In the present invention, the fourth mixing is preferably firstly stirring at a low speed and then stirring at a high speed; the rate of the low-speed stirring is preferably 130-150rpm, more preferably 140rpm; the time of the low-speed stirring is preferably 1-2min, more preferably 1min; the rate of the high-speed stirring is preferably 270-300rpm, more preferably 290rpm; the time of the high-speed stirring is preferably 2-3min, more preferably 2min; the equipment used for the fourth mixing is preferably a stirring pot; after the high-speed stirring, the present invention preferably uses a spatula to scrape the unmixed materials on the pot wall and blades of the stirring pot into the stirred materials in the stirring pot. In the fourth mixing process, the low-speed stirring is first used to make the dry material fully contact with the liquid, and at the same time, it can also prevent the material from splashing out during high-speed stirring.
[0071] In the present invention, the mixing and dispersion of the mixture and the fibers are preferably performed as follows: under low-speed stirring, the fibers are gradually added to the mixture, and then high-speed stirring is performed for dispersion; the gradual addition is preferably performed in small amounts and multiple times; the low-speed stirring rate is preferably 130-150 rpm, more preferably 140 rpm; the high-speed stirring rate is preferably 270-300 rpm, more preferably 290 rpm; the high-speed stirring time is preferably 3-5 min, more preferably 5 min; the present invention preferably manually disperses the clumped fibers and then adds them to the mixture to prevent the fibers from clumping.
[0072] The present invention also provides the use of the non-expanding fire retardant coating described in the above technical solution or the non-expanding fire retardant coating prepared by the preparation method described in the above technical solution in fire prevention of fiber reinforced composite materials.
[0073] The present invention also provides a non-expansion fire retardant coating, comprising the following steps: coating the non-expansion fire retardant coating on the surface of the fiber-reinforced composite material, and then performing curing to obtain the non-expansion fire retardant coating;
[0074] The non-expanding fire retardant coating is the non-expanding fire retardant coating described in the above technical solution or the non-expanding fire retardant coating prepared by the preparation method described in the above technical solution.
[0075] In the present invention, the coating method is preferably manual application or spraying, more preferably manual application; the curing temperature is preferably 25-35°C, more preferably 25-30°C; the curing humidity is preferably 70-85%, more preferably 70-80%; the curing time is preferably 14-28d, more preferably 28d. The present invention does not specifically limit the thickness of the non-expanding fire retardant coating, which can be determined according to the requirements of the use scenario. In the application example of the present invention, the thickness of the non-expanding fire retardant coating is 25mm.
[0076] The technical solutions of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention, but they should not be construed as limiting the protection scope of the present invention.
[0077] Example 1
[0078] The raw materials for preparing the non-expanding fire retardant coating described in Example 1 are shown in Table 1:
[0079] Table 1 Preparation materials of the non-expandable fire retardant coating described in Example 1
[0080]
[0081] Among them, the D50 particle size of kaolin is 9.1μm; the D50 particle size of fly ash is 5.2μm; the water glass activator is a mixed solution of sodium silicate and sodium hydroxide; the modulus of the water glass activator is 1.6M; the particle size of the redispersible latex powder is 5μm; the particle size of the polyvinyl alcohol powder is 120 mesh, and the number average molecular weight of the polyvinyl alcohol powder is 80000; the D50 particle size of the expanded vermiculite is 226.6μm; the particle size of the vitrified microsphere is The diameter is 1-2 mm; the particle size of sepiolite is 350-400 μm; the hollow glass microspheres are composed of two types of hollow glass microspheres with a particle size of D50 = 65 μm and a particle size of D50 = 40 μm, the volume ratio of the two types of hollow glass microspheres with a particle size of D50 = 65 μm and a particle size of D50 = 40 μm is 7:3, the wall thickness of the hollow glass microspheres is 2 μm, and the true density of the hollow glass microspheres with a particle size of D50 = 40 μm is 0.6 g / cm 3 , bulk density is 0.35g / cm 3 The true density of hollow glass microspheres with a particle size of D50 = 65 μm is 0.2 g / cm 3 , bulk density is 0.1g / cm 3 , the length of the glass fiber is 6mm and the diameter is 15μm; the foaming agent is sodium a-olefin sulfonate; the foam stabilizer is calcium stearate and commercial powder foam stabilizer (Luoyang Tongrun Nano Technology Co., Ltd., model: lightweight partition board foam stabilizer) in a mass ratio of 1:1; the thickener is sodium hydroxymethyl cellulose and cellulose ether in a mass ratio of 1:1;
[0082] The preparation method of the non-expandable fire retardant coating is as follows:
[0083] Step 1: First, add the binder except the water glass activator, the heat insulation filler except the hollow glass microspheres, and the flame retardant into a stirring pot for dry mixing, and stir at a low speed of 140 rpm for 3 minutes to obtain a base material;
[0084] Step 2: Add a foaming agent, a thickener and a foam stabilizer to the base material, continue stirring at a low speed of 140 rpm for 1 minute, and use a cover plate to cover the top of the stirring pot to prevent the added additives from splashing out to obtain a dry material;
[0085] Step 3: Add hollow glass microspheres to the dry material. Due to its extremely low density, first use manual stirring to disperse it in the dry material, and then stir it at a low speed of 140 rpm for 1 minute. It also needs to be covered with a cover plate to obtain a hollow glass microsphere mixture;
[0086] Step 4: Mix the acrylic emulsion and water and stir evenly at 30 rpm to obtain a mixed solution of acrylic emulsion and water;
[0087] Step 5: Add the water glass activator and the mixture of acrylic emulsion and water into the hollow glass microbead mixture in the stirring pot, first stir at a low speed of 140rpm for 1min to allow the dry material to fully contact the liquid and prevent the material from splashing out during high-speed stirring, then stir at a high speed of 290rpm for 2min, and use a spatula to scrape the unmixed materials on the wall and blades of the stirring pot into the mixed materials in the stirring pot to obtain a mixture;
[0088] Step 6: Add glass fiber to the mixture at a low speed of 140 rpm. When adding glass fiber, add it gradually in small amounts and multiple times, and manually disperse the clumped fibers before adding them, and stir again at a high speed of 290 rpm for 5 minutes to fully disperse the fibers in the slurry to obtain a non-expanding fire retardant coating.
[0089] Example 2
[0090] The difference from Example 1 is that the amount of the thermal insulation filler in Example 1 is replaced with 13.4% of the mass of the non-expanding fire retardant coating.
[0091] Example 3
[0092] The difference from Example 1 is that the glass fiber in Example 1 is replaced by carbon fiber.
[0093] Comparative Example 1
[0094] The difference from Example 1 is that no hollow glass microspheres are added.
[0095] Comparative Example 2
[0096] The difference from Example 1 is that no foaming agent is added.
[0097] Comparative Example 3
[0098] The difference from Example 1 is that no flame retardant is added.
[0099] Application Example 1
[0100] The non-expanding fire retardant coating prepared in Example 1 was applied to the surface of the reinforcement made of fiber-reinforced composite material by manual coating, and cured at 25° C. and 70% humidity for 28 days to obtain a non-expanding fire retardant coating with a thickness of 25 mm.
[0101] Application Example 2
[0102] The difference from Application Example 1 is that the non-expanding fire retardant coating prepared in Example 1 is replaced by the non-expanding fire retardant coating prepared in Example 2, and the rest of the contents are consistent with Application Example 1.
[0103] Application Example 3
[0104] The difference from Application Example 1 is that the non-expanding fire retardant coating prepared in Example 1 is replaced by the non-expanding fire retardant coating prepared in Example 3, and the rest of the contents are consistent with Application Example 1.
[0105] Comparative application example 1
[0106] The difference from Application Example 1 is that the non-expanding fire retardant coating prepared in Example 1 is replaced by the non-expanding fire retardant coating prepared in Comparative Example 1, and the rest of the contents are consistent with Application Example 1.
[0107] Comparative Application Example 2
[0108] The difference from Application Example 1 is that the non-expanding fire retardant coating prepared in Example 1 is replaced by the non-expanding fire retardant coating prepared in Comparative Example 2, and the rest of the contents are consistent with Application Example 1.
[0109] Comparative Application Example 3
[0110] The difference from Application Example 1 is that the non-expanding fire retardant coating prepared in Example 1 is replaced by the non-expanding fire retardant coating prepared in Comparative Example 3, and the rest of the contents are consistent with Application Example 1.
[0111] Performance Testing
[0112] (1) The density of the coating formed by the non-intumescent fire retardant coating prepared in Examples 1 and 2 was tested. The specific test method was as follows: a 50 mm × 50 mm × 50 mm cube was used to measure the dry density. After curing for 28 days, the specimen was placed in a drying oven at 105° C. and dried to constant weight. The side length b was then measured with a vernier caliper. The mass m was then weighed. The density was calculated using the following formula:
[0113]
[0114] The density of the coating formed by the non-intumescent fire retardant coating prepared in Examples 1 and 2 of the present invention is 560 kg / m 3 and 730kg / m 3 .
[0115] (2) The compressive strength of the coating formed by the non-expanding fire retardant coating prepared in Example 1 was tested. Specifically, the compressive strength test was also carried out using a 50 mm × 50 mm × 50 mm cube. After curing for 28 days, it was placed in a drying oven at 60° C. for 12 hours, and then a 5 t MTS testing machine was used for the compressive test. The loading rate was 200 N / min. The compressive test was as follows: Figure 1 shown.
[0116] The compressive strength of the coating formed by the non-expanding fire retardant coating prepared by the present invention is 0.66MPa.
[0117] (3) The flexural strength of the coating formed by the non-intumescent fire retardant coating prepared in Example 1 was tested. Specifically, the flexural strength test was performed using a 160 mm × 40 mm × 40 mm test piece, which was placed in a drying oven at 60° C. for 12 h after curing for 28 days, and then subjected to a flexural test using a standard compression flexural test machine at a loading rate of 10 mm / min. Figure 2 shown.
[0118] The flexural strength of the coating formed by the non-expanding fire retardant coating prepared by the present invention is 0.49 MPa.
[0119] (4) Bond strength: The bond strength in the present invention refers to the bond strength between the coating formed by the non-expanding fire retardant coating prepared in Example 1 and the cement mortar substrate. A 70 mm × 70 mm × 20 mm cement mortar test block was used and a 5 mm thick coating was applied on the surface of the test block. After curing for 28 days, the bond strength was tested by a direct pull test. The bond strength direct pull test is as follows: Figure 3 shown.
[0120] The bonding strength of the coating formed by the non-expanding fire retardant coating prepared by the present invention is 0.2MPa.
[0121] (5) Water resistance: A fiber-reinforced low-alkalinity cement building slab was used as the base plate, with a size of 150 mm × 70 mm × 6 mm. A 5 mm thick non-expanding fire retardant coating prepared in Example 1 was applied to the surface of the base plate to form a coating. After curing for 28 days, the edges and back of the specimen were sealed with a mixed solution of paraffin and rosin (mass ratio of 1:1). Then 2 / 3 of the specimen was immersed in water. After immersion in water for 28 days, no cracks appeared on the surface. The water resistance test was as follows: Figure 4 shown.
[0122] (6) High and low temperature cycle: The specimens used in the high and low temperature resistance test are the same as those used in the water resistance test. The cycle process is as follows: store them in an environment of -20℃±2℃ for 3 hours, then store them in an environment of 50℃±2℃ for 3 hours, and repeat the above process 20 times.
[0123] The non-expanding fire-retardant coating prepared by the present invention has no surface cracks after 20 cycles.
[0124] (7) Fire resistance: A simplified version of the fire resistance limit test was used. The test substrate was a 150mm×150mm×25mm concrete block. A 25mm thick layer of non-expanding fire retardant coating prepared in Example 1 was applied on the surface, and the surface was smoothed and then cured for 28 days. The test equipment used was a multifunctional box furnace purchased by the laboratory. The equipment can achieve a heating process close to that described by the ISO standard heating curve. During the test, the coating surface was facing the inside of the furnace and directly exposed to the high temperature environment. The temperature change at the interface between the coating and the concrete substrate was then recorded by a thermocouple pre-buried in the specimen. The test schematic is shown in the figure. Figure 5 As shown, the results are Figure 6 The furnace temperature refers to the temperature of the high-temperature furnace cavity, which is also the temperature applied to the coating surface. The temperature at the interface between the coating and the substrate is also the temperature of the FRP material, and the FRP is attached to the surface of the substrate.
[0125] In the fire resistance test, the temperature change of the back side of the coating under fire was recorded. Figure 6 It can be seen that there is an obvious platform section in the temperature curve in the early stage of fire, which is very conducive to the FRP reinforcement system to continue to play a reinforcing role under fire, so as not to be damaged in a short time after the fire. This provides more sufficient time for people to escape and rescue under fire, and can effectively reduce the harm and losses caused by fire.
[0126] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention rather than all the embodiments. People can also obtain other embodiments based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.
Claims
1. A non-expanding fire retardant coating, characterized in that: The raw materials include binder, thermal insulation filler, flame retardant, fiber, additives and water: The binder comprises metakaolin, fly ash and an activator; The heat-insulating filler includes expanded vermiculite, vitrified microspheres, sepiolite and hollow glass microspheres; The flame retardant includes aluminum hydroxide and magnesium hydroxide; The fibers include glass fibers and / or carbon fibers; The auxiliary agents include a foaming agent, a thickener, a foam stabilizer and acrylic emulsion.
2. The non-intumescent fire retardant coating according to claim 1, characterized in that: The hollow glass microspheres include two types of hollow glass microspheres with a D50 particle size of 65 μm and a D50 particle size of 40 μm; the volume ratio of the two types of hollow glass microspheres with a D50 particle size of 65 μm and a D50 particle size of 40 μm is 7:
3.
3. The non-intumescent fire retardant coating according to claim 1, characterized in that: The mass of the flame retardant is 2.3-8.2% of the mass of the non-expanding fire retardant coating; the mass ratio of the aluminum hydroxide to the magnesium hydroxide is 1.5-2.5:
1.
4. The non-intumescent fire retardant coating according to claim 1, characterized in that: The foaming agent includes sodium α-olefin sulfonate.
5. The non-expanding fire retardant coating according to claim 1, characterized in that: The foam stabilizer includes calcium stearate and / or a commercial powder foam stabilizer.
6. The non-expanding fire retardant coating according to claim 1, characterized in that: The thickener includes sodium hydroxymethylcellulose and / or cellulose ether.
7. The non-intumescent fire retardant coating according to claim 1, characterized in that: The mass ratio of the metakaolin to the fly ash is 5-7:3-5.
8. The method for preparing the non-intumescent fire retardant coating according to any one of claims 1 to 7, characterized in that: The following steps are involved: A binder other than the activator, a heat-insulating filler other than the hollow glass microspheres, and a flame retardant are first mixed to obtain a base material; The base material, foaming agent, thickener and foam stabilizer are mixed for the second time to obtain a dry material; The dry material and hollow glass microspheres are mixed for a third time, and then an activator, acrylic emulsion and water are added for a fourth mixing to obtain a mixture; The mixed material and the fibers are mixed and dispersed to obtain a non-expanding fire retardant coating.
9. Use of the non-expanding fire retardant coating according to any one of claims 1 to 7 or the non-expanding fire retardant coating prepared by the preparation method according to claim 8 in fire protection of fiber-reinforced composite materials.
10. A method for preparing a non-intumescent fire retardant coating, characterized in that: The following steps are involved: After coating the non-expanding fire retardant coating on the surface of the fiber-reinforced composite material, curing is performed to obtain the non-expanding fire retardant coating; The non-expanding fire retardant coating is the non-expanding fire retardant coating according to any one of claims 1 to 7 or the non-expanding fire retardant coating prepared by the preparation method according to claim 8.
Citation Information
Patent Citations
Thin fire-resistant / flame-retardant paint for tunnel and preparation method thereof
CN103043976A
Alkali slag tunnel fireproof coating and use method thereof
CN104194426A
Alkaline ore slag tunnel fireproof coating using composite activator and preparation method thereof
CN107117878A
Cement-based steel structure fireproof coating and preparation method thereof
CN118085619A
Cited By
Environment-friendly inorganic expansible fireproof coating and preparation method thereof
CN119432132A