Graphene oxide and siloxane polymer composite modified geopolymer anticorrosive paint as well as preparation method and application thereof
By combining graphene oxide with silicone polymer modified polymer anticorrosion coating, the existing coating materials are easily aging and poor weather resistance, achieving high corrosion resistance and long service life of the coating, and reducing the coating's high corrosion resistance and long service life. Discharge of hazardous substances.
Patent Information
- Application Number
- CN202411337520.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-25
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-09-25
AI Technical Summary
Existing coating materials are prone to aging in reinforced bars and concrete structures, poor weather resistance, and produce harmful volatile organic compounds during production and construction, affecting the durability and environmental protection performance of the structure.
Using graphene oxide and silicone polymer composite modified polymer anticorrosion coating, the hydrophobicity and durability of the coating are enhanced by the hydrophobic modifier and silane coupling agent of the silicone polymer to form covalent bonds. To improve mechanical properties and waterproof performance.
It significantly improves the corrosion resistance and service life of the coating, reduces the risk of invasion of water molecules carrying harmful ions, reduces the aging and weather resistance of the coating, and reduces the emission of harmful substances.
Smart Images

Figure BDA0005058685390000021 
Figure BDA0005058685390000041 
Figure BDA0005058685390000101
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of anti-corrosion materials, and specifically relates to a graphene oxide and siloxane polymer composite modified geopolymer anti-corrosion coating, and a preparation method and application thereof. Background Art
[0002] In the long-term use of modern buildings and infrastructure, water, as the main carrier of harmful ions, is a key factor in inducing steel corrosion and concrete structure deterioration. The most widely used coating materials such as epoxy resin, polyurethane, and acrylic have good chemical resistance, impermeability, and anti-corrosion properties. However, problems such as low mechanical strength, easy aging, and poor weather resistance of the coatings lead to the need for frequent repair or replacement of the coatings. In addition, these materials produce volatile organic compounds (VOCs) during production and construction, which are potentially harmful to the atmosphere and human health. Therefore, the development of more durable and environmentally friendly coating materials has become the primary link to improve the durability and protective properties of concrete and steel structures. Geopolymer is an inorganic polymer, which is usually synthesized by alkaline activation of aluminosilicate precursors. The special aluminosilicate network structure formed during the hardening process is conducive to coating and protecting the substrate surface. Geopolymer generally has high mechanical strength, good chemical stability, and compactness. In addition, geopolymer is a sustainable cementitious material that can reduce CO2 footprint. Although the patent CN118240403A proposes that the addition of graphene oxide to geopolymer can establish a highly dense polymer network system and improve the interfacial bonding ability between the coating and the steel, the graphene oxide-geopolymer coating is still a hydrophilic material, which makes it susceptible to water intrusion, seriously affecting the corrosion resistance and service life of the geopolymer coating. Summary of the invention
[0003] In view of this, the object of the present invention is to provide a graphene oxide and siloxane polymer composite modified geopolymer anti-corrosion coating and a preparation method and application thereof. The graphene oxide and siloxane polymer composite modified geopolymer anti-corrosion coating provided by the present invention has strong corrosion resistance and long service life.
[0004] In order to achieve the above object, the present invention provides the following technical solutions:
[0005] The present invention provides a graphene oxide and siloxane polymer composite modified geopolymer anticorrosion coating, wherein the raw materials for preparation include the following components in parts by mass:
[0006] 140-160 parts of aluminosilicate minerals,
[0007] 95-105 parts of alkali activator,
[0008] 0.05-0.2 parts of graphene oxide,
[0009] Surfactant 0.05-0.2 parts,
[0010]
[0011] Preferably, the specific surface area of the graphene oxide is 100 to 400 m 2 / g; the number of layers of the graphene oxide is 1 to 2 layers; and the sheet diameter of the graphene oxide is 0.2 to 10 μm.
[0012] Preferably, the siloxane polymer is polydimethylsiloxane.
[0013] Preferably, the silane coupling agent is silane coupling agent KH550.
[0014] Preferably, the alkaline activator comprises sodium hydroxide, water and water glass; the modulus of the alkaline activator is 1.3-2M.
[0015] Preferably, the aluminosilicate minerals include one or more of fly ash, slag and metakaolin.
[0016] The present invention also provides a method for preparing the graphene oxide and siloxane polymer composite modified geopolymer anticorrosion coating described in the above technical solution, comprising the following steps:
[0017] first mixing a portion of the alkaline activator, graphene oxide and a surfactant to obtain a graphene oxide dispersion;
[0018] The siloxane polymer, the silane coupling agent and the remaining base activator are mixed and hydrolyzed to obtain a hydrophobic modifier;
[0019] The graphene oxide dispersion, the organosilicon defoamer, the hydrophobic modifier, the aluminosilicate mineral, the polyvinyl alcohol powder and the titanium dioxide are thirdly mixed to obtain a graphene oxide and siloxane polymer composite modified geopolymer anticorrosive coating.
[0020] The present invention also provides the use of the graphene oxide and siloxane polymer composite modified geopolymer anti-corrosion coating described in the above technical scheme or the graphene oxide and siloxane polymer composite modified geopolymer anti-corrosion coating prepared by the preparation method described in the above technical scheme in steel corrosion protection.
[0021] The present invention also provides a method for preparing a hydrophobic geopolymer inorganic anticorrosive coating, comprising the following steps:
[0022] The graphene oxide and siloxane polymer composite modified geopolymer anti-corrosion coating is applied on the surface of steel and dried to obtain a hydrophobic geopolymer inorganic anti-corrosion coating;
[0023] The graphene oxide and siloxane polymer composite modified geopolymer anti-corrosion coating is the graphene oxide and siloxane polymer composite modified geopolymer anti-corrosion coating according to any one of claims 1 to 6 or the graphene oxide and siloxane polymer composite modified geopolymer anti-corrosion coating prepared by the preparation method according to claim 7.
[0024] Preferably, the coating is spraying; the diameter of the spraying nozzle is 2-4 mm; the spraying pressure is 3-5 MPa; the distance between the spraying nozzle and the steel is 12-18 cm; the spraying time is 10-15 s; the spraying coating amount is 0.2-0.3 g / cm 2 .
[0025] The invention provides a graphene oxide and siloxane polymer composite modified geopolymer anticorrosive coating. The raw materials for preparing the coating include the following components, measured by weight: 140-160 parts of aluminosilicate minerals, 95-105 parts of alkali activators, 0.05-0.2 parts of graphene oxide, 0.05-0.2 parts of surfactants, 3-9 parts of siloxane polymers, 0.15-0.6 parts of silane coupling agents, 2-4 parts of polyvinyl alcohol powders, 7-8 parts of titanium dioxide and 0.7-0.8 parts of organosilicon defoaming agents.
[0026] The present invention uses siloxane polymer as the main hydrophobic agent and silane coupling agent as the auxiliary hydrophobic agent, and improves the hydrophobicity and durability of the geopolymer coating by hydrophobically modifying the graphene oxide-geopolymer coating. Siloxane polymer has excellent chemical stability, high adhesion and outstanding water resistance. It has a Si-O-Si main chain structure and a CH3 hydrophobic group. It can be cross-linked with the silicon-oxygen tetrahedron and aluminum-oxygen tetrahedron structure in the geopolymer through chemical reaction to form a covalent bond, thereby enhancing the mechanical properties, hydrophobicity and durability of the geopolymer. As an auxiliary modifier, the silane coupling agent can ensure that the siloxane polymer has good compatibility with the geopolymer matrix, thereby optimizing and enhancing the performance without significantly affecting the original characteristics of the geopolymer, thereby effectively improving the anti-corrosion performance and service life of the coating.
[0027] The present invention also provides a method for preparing the above-mentioned graphene oxide and siloxane polymer composite modified geopolymer anti-corrosion coating. The present invention prepares the raw materials by adding and mixing in steps, so that the components are evenly dispersed and fully reacted, which can effectively improve the long-term corrosion resistance of the coating. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 The contact angle diagram of the coated steel bars prepared in Application Examples 1 to 3 and the coated steel bars in Comparative Application Example 1;
[0029] Figure 2The results of salt spray corrosion tests on the coated steel bars prepared in Application Examples 1 to 3, the coated steel bars in Comparative Application Example 1, and the uncoated steel bars are shown. DETAILED DESCRIPTION
[0030] The present invention provides a graphene oxide and siloxane polymer composite modified geopolymer anticorrosion coating, wherein the raw materials for preparation include the following components in parts by mass:
[0031] 140-160 parts of aluminosilicate minerals,
[0032] 95-105 parts of alkali activator,
[0033] 0.05-0.2 parts of graphene oxide,
[0034] Surfactant 0.05-0.2 parts,
[0035] 3 to 9 parts of siloxane polymer,
[0036]
[0037] Unless otherwise specified, the present invention has no special requirements on the sources of the raw materials used in the preparation, and commercially available products known to those skilled in the art can be used.
[0038] The raw materials for preparing the graphene oxide and siloxane polymer composite modified geopolymer anti-corrosion coating provided by the present invention include 140 to 160 parts by mass of aluminosilicate minerals, preferably 145 to 150 parts. In the present invention, the aluminosilicate minerals preferably include one or more of fly ash, slag and metakaolin, more preferably fly ash, slag and metakaolin; the mass ratio of the fly ash, slag and metakaolin is preferably 70 to 80:40 to 50:25 to 35, more preferably 75:45:30; the calcium content of the fly ash is preferably 3 to 10%, more preferably 5%; the particle size of the fly ash is preferably 1.6 to 64.3 μm, more preferably 1.98 to 61.1 μm; the content of the slag is preferably 1.6 to 64.3 μm, more preferably 1.98 to 61.1 μm; the content of the slag is preferably 1.6 to 64.3 μm, more preferably 1.98 to 61.1 μm. The calcium content is preferably 40-50%, more preferably 45-47%; the particle size of the slag is preferably 2.1-49.8 μm, more preferably 2.2-46.8 μm; the metakaolin is preferably obtained by calcining kaolin; the calcination temperature is preferably 600-900°C, more preferably 700-800°C, and the insulation time is preferably 30-60 min, more preferably 40-60 min; the particle size of the metakaolin is preferably 0.2-6.3 μm, more preferably 0.22-5.4 μm.
[0039] Based on 1 mass part of aluminosilicate mineral, the raw materials for preparing the graphene oxide and siloxane polymer composite modified geopolymer anticorrosive coating provided by the present invention include 95 to 105 mass parts of alkali activator, preferably 96 to 104 mass parts. In the present invention, the alkali activator preferably includes sodium hydroxide, water and water glass; the modulus of the alkali activator is preferably 1.3 to 2M, more preferably 1.4 to 1.5M; the water is preferably deionized water; the modulus of the water glass is preferably 2 to 2.5M, more preferably 2.2 to 2.4M; the mass ratio of the sodium hydroxide, water and water glass is preferably 3.5 to 4.5:35 to 45:55 to 65, more preferably 4:40:60.
[0040] In the present invention, the preparation method of the alkaline activator preferably comprises the following steps: dissolving sodium hydroxide in water to obtain a sodium hydroxide solution; mixing the sodium hydroxide solution with water glass and allowing to stand to obtain an alkaline activator; the mixing is preferably carried out under stirring; the stirring rate is preferably 200 to 800 rpm, more preferably 400 to 800 rpm; the stirring time is preferably 5 to 10 min, more preferably 8 to 10 min; the standing time is preferably 18 to 26 h, more preferably 24 h.
[0041] The raw material for preparing the graphene oxide and siloxane polymer composite modified geopolymer anticorrosive coating provided by the present invention comprises 0.05 to 0.2 parts by mass of graphene oxide, preferably 0.1 to 0.15 parts by mass, based on 1 part by mass of aluminosilicate mineral. In the present invention, the specific surface area of the graphene oxide is preferably 100 to 400 m 2 / g, more preferably 200 to 400 m 2 / g; the number of layers of the graphene oxide is preferably 1 to 2 layers, more preferably 1 layer; the sheet diameter of the graphene oxide is preferably 0.2 to 10 μm, more preferably 0.2 to 5 μm.
[0042] Graphene oxide is a carbon-based nanomaterial with a high aspect ratio, high specific surface area and elastic modulus. The surface of graphene oxide has many oxygen functional groups, including hydroxyl (-OH), carboxyl (-COOH) and epoxy (-COOC). These groups help graphene oxide to interact with geopolymer gel molecules and the oxide film on the surface of steel, effectively compacting the microstructure of the geopolymer, improving the inherent high brittleness of the geopolymer, and improving the interfacial bonding ability between the geopolymer and the steel, thereby enhancing the anti-corrosion performance of geopolymer-coated steel bars.
[0043] The raw materials for preparing the graphene oxide and siloxane polymer composite modified geopolymer anticorrosive coating provided by the present invention include 0.05 to 0.2 parts by mass of surfactant, preferably 0.1 to 0.15 parts by mass, based on 1 part by mass of aluminosilicate mineral. In the present invention, the surfactant is preferably a polycarboxylate water reducer, sodium lauryl sulfate or polyethylene glycol; more preferably a polycarboxylate water reducer.
[0044] The raw materials for preparing the graphene oxide and siloxane polymer composite modified geopolymer anticorrosive coating provided by the present invention include 3 to 9 parts by mass of siloxane polymer, preferably 3 to 6 parts by mass, based on 1 part by mass of aluminosilicate mineral. In the present invention, the siloxane polymer is preferably polydimethylsiloxane; the number average molecular weight of the siloxane polymer is preferably 10,000 to 100,000, more preferably 20,000 to 80,000.
[0045] Siloxane polymers have excellent chemical stability, high adhesion and outstanding waterproof properties. Siloxane polymers have a Si-O-Si main chain structure and a CH3 hydrophobic group, which can cross-link with the silicon-oxygen tetrahedron and aluminum-oxygen tetrahedron structures in geopolymers through chemical reactions to form covalent bonds, thereby enhancing the mechanical properties, hydrophobicity and durability of the geopolymers, and making the coating have excellent corrosion resistance and service life.
[0046] Polydimethylsiloxane (PDMS) is a silicone polymer composed of Si-O chains and hydrophobic methyl groups (-CH3), which has excellent chemical stability, high adhesion and outstanding water resistance. The geopolymer coating is modified by composite modification of graphene oxide and polydimethylsiloxane to form a hydrophobic barrier on the surface and in the matrix, thereby reducing water absorption and minimizing the risk of degradation associated with harmful ions.
[0047] The raw materials for preparing the graphene oxide and siloxane polymer composite modified geopolymer anticorrosive coating provided by the present invention include 0.15 to 0.6 parts by mass of a silane coupling agent, preferably 0.3 to 0.5 parts by mass, based on 1 part by mass of aluminosilicate mineral. In the present invention, the silane coupling agent is preferably silane coupling agent KH550.
[0048] As an auxiliary modifier, silane coupling agent can ensure the good compatibility of siloxane polymer with geopolymer matrix, thereby optimizing and enhancing the performance without significantly affecting the original properties of geopolymer, so that the coating has excellent corrosion resistance and service life.
[0049] The raw materials for preparing the graphene oxide and siloxane polymer composite modified geopolymer anticorrosive coating provided by the present invention include 2 to 4 parts by mass of polyvinyl alcohol powder, preferably 3 parts, based on 1 part by mass of aluminosilicate mineral. In the present invention, the molecular weight of polyvinyl alcohol in the polyvinyl alcohol powder is preferably 100000 to 124000Mn, more preferably 117000 to 122000Mn; the particle size of the polyvinyl alcohol powder is preferably 100 to 110 μm, more preferably 100 to 105 μm.
[0050] The raw materials for preparing the graphene oxide and siloxane polymer composite modified geopolymer anticorrosive coating provided by the present invention include 7 to 8 parts by mass of titanium dioxide, preferably 7.5 parts, based on 1 part by mass of aluminosilicate mineral. In the present invention, the titanium dioxide is preferably titanium dioxide for architectural coatings, the main component of which is rutile titanium dioxide; the particle size of the titanium dioxide is preferably 0.04 to 2.6 μm, more preferably 0.06 to 1.8 μm.
[0051] The raw materials for preparing the graphene oxide and siloxane polymer composite modified geopolymer anticorrosive coating provided by the present invention include 0.7 to 0.8 parts by mass of an organosilicon defoamer, preferably 0.75 parts, based on 1 part by mass of aluminosilicate mineral. In the present invention, the organosilicon defoamer is preferably a silicone oil type defoamer.
[0052] The present invention also provides a method for preparing the graphene oxide and siloxane polymer composite modified geopolymer anticorrosion coating described in the above technical solution, comprising the following steps:
[0053] first mixing a portion of the alkaline activator, graphene oxide and a surfactant to obtain a graphene oxide dispersion;
[0054] The siloxane polymer, the silane coupling agent and the remaining base activator are mixed and hydrolyzed to obtain a hydrophobic modifier;
[0055] The graphene oxide dispersion, the organosilicon defoamer, the hydrophobic modifier, the aluminosilicate mineral, the polyvinyl alcohol powder and the titanium dioxide are thirdly mixed to obtain a graphene oxide and siloxane polymer composite modified geopolymer anticorrosive coating.
[0056] The present invention first mixes part of the alkali activator, graphene oxide and a surfactant to obtain a graphene oxide dispersion.
[0057] In the present invention, the first mixing is preferably adding graphene oxide to an alkali activator for a first stirring, then adding a surfactant for a second stirring, and finally performing ultrasonic dispersion; the first stirring rate is preferably 200-800rpm, more preferably 500-800rpm; the first stirring time is preferably 1-2min, more preferably 1min; the second stirring rate is preferably 800-1400rpm, more preferably 1000-1200rpm; the second stirring time is preferably 3-5min, more preferably 4min; the ultrasonic dispersion power is preferably 100-400W, more preferably 120-300W; the ultrasonic dispersion time is preferably 60-90min, more preferably 60-70min.
[0058] The present invention performs a second mixing of siloxane polymer, silane coupling agent and residual alkali activator for hydrolysis to obtain a hydrophobic modifier.
[0059] In the present invention, the second mixing is preferably adding the siloxane polymer and the silane coupling agent to the remaining base activator in sequence; the hydrolysis is preferably carried out under stirring; the stirring rate is preferably 800-1400rpm, more preferably 1000-1200rpm; the stirring time is preferably 5-10min, more preferably 7-10min.
[0060] After obtaining the graphene oxide dispersion and the hydrophobic modifier, the present invention thirdly mixes the graphene oxide dispersion, the silicone defoamer, the hydrophobic modifier, the aluminosilicate mineral, the polyvinyl alcohol powder and the titanium dioxide to obtain a graphene oxide and siloxane polymer composite modified geopolymer anticorrosive coating.
[0061] In the present invention, the third mixing is preferably mixing aluminosilicate minerals, rubber powder polyvinyl alcohol powder and titanium dioxide for a third stirring to obtain a mixed powder; pouring the graphene oxide dispersion and the silicone defoamer into the mixed powder for a fourth stirring, and then adding the hydrophobic modifier for a fifth stirring; the rate of the third stirring is preferably 30 to 60 rpm, more preferably 40 to 60 rpm; the time of the third stirring is preferably 2 to 4 min, more preferably 2 to 3 min; the rate of the fourth stirring is preferably 60 to 100 rpm, more preferably 80 to 100 rpm; the time of the fourth stirring is preferably 1 to 2 min, more preferably 2 min; the rate of the fifth stirring is preferably 60 to 100 rpm, more preferably 80 to 100 rpm; the time of the fifth stirring is preferably 1 to 3 min, more preferably 2 min.
[0062] The present invention also provides the use of the graphene oxide and siloxane polymer composite modified geopolymer anti-corrosion coating described in the above technical scheme or the graphene oxide and siloxane polymer composite modified geopolymer anti-corrosion coating prepared by the preparation method described in the above technical scheme in steel corrosion protection.
[0063] The present invention also provides a method for preparing a hydrophobic geopolymer inorganic anticorrosive coating, comprising the following steps:
[0064] The graphene oxide and siloxane polymer composite modified geopolymer anti-corrosion coating is applied on the surface of steel and dried to obtain a hydrophobic geopolymer inorganic anti-corrosion coating;
[0065] The graphene oxide and siloxane polymer composite modified geopolymer anti-corrosion coating is the graphene oxide and siloxane polymer composite modified geopolymer anti-corrosion coating described in the above technical solution or the graphene oxide and siloxane polymer composite modified geopolymer anti-corrosion coating prepared by the preparation method described in the above technical solution.
[0066] In the present invention, the coating is preferably spraying; the diameter of the spraying nozzle is preferably 2-4 mm, more preferably 3 mm; the spraying pressure is preferably 3-5 MPa, more preferably 4 MPa; the distance between the spraying nozzle and the steel is preferably 12-18 cm, more preferably 15 cm; the spraying time is preferably 10-15 s, more preferably 10-12 s; the spraying coating amount is preferably 0.2-0.3 g / cm 2 , more preferably 0.25 g / cm 2 ; The drying temperature is preferably 20-25°C, more preferably 22°C; the drying time is preferably 40-60min, more preferably 50-60min; the thickness of the hydrophobic geopolymer inorganic anti-corrosion coating is preferably 180-200μm, more preferably 200μm.
[0067] The technical solutions of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention, but they should not be construed as limiting the protection scope of the present invention.
[0068] Example 1
[0069] Dissolve 4 g of sodium hydroxide in 40 g of deionized water to obtain a sodium hydroxide solution; mix the sodium hydroxide solution with 60 g of water glass with a modulus of 2.2 M, stir at 400 rpm for 10 min, and let stand for 24 h to obtain a 1.5 M alkali activator;
[0070] 0.1125 g of graphene oxide (with a specific surface area of 400 m 2 / g, the number of layers is 1 layer, and the sheet diameter is 0.2 μm) is mixed with 94 g of an alkali activator and stirred at 800 rpm for 1 min in a magnetic stirrer, and then 0.1125 g of a surfactant (polycarboxylate water reducer) is added to improve the dispersibility of graphene oxide, and stirring is continued at 800 rpm for 4 min. Finally, it is ultrasonically dispersed at a power of 120 W for 60 min to obtain a graphene oxide dispersion;
[0071] 3 g of polydimethylsiloxane (number average molecular weight of 80,000) and 0.15 g of silane coupling agent (KH550) were sequentially added to 10 g of the base activator, and stirred in a magnetic stirrer at 1000 rpm for 10 min to fully hydrolyze, thereby obtaining a hydrophobic modifier;
[0072] Weigh 75g of fly ash (calcium content of 5%, particle size of 50μm), 45g of slag (calcium content of 47%, particle size of 10μm), 30g of metakaolin (calcined kaolin, calcined at 800℃, holding time of 60min, particle size of 5μm), 3g of polyvinyl alcohol powder (particle size of 100μm, number average molecular weight of 100,000Mn), 7.5g of titanium dioxide (particle size of 1μm, titanium dioxide for architectural coatings, its main components The mixture was poured into a stirring container and stirred at 60 rpm for 2 min to obtain a mixed powder. Subsequently, the graphene oxide dispersion and 0.75 g of an organosilicon defoamer (silicone oil defoamer) were poured into the mixed powder and stirred at 100 rpm for 2 min. Finally, a hydrophobic modifier was added and stirred at 100 rpm for 2 min to obtain a composite modified geopolymer anticorrosion coating of graphene oxide and siloxane polymer.
[0073] Example 2
[0074] The difference from Example 1 is that 3 g of polydimethylsiloxane and 0.15 g of silane coupling agent (KH550) in Example 1 are replaced by 6 g of polydimethylsiloxane emulsion and 0.3 g of silane coupling agent KH550.
[0075] Example 3
[0076] The difference from Example 1 is that 3 g of polydimethylsiloxane and 0.15 g of silane coupling agent (KH550) in Example 1 are replaced by 9 g of polydimethylsiloxane emulsion and 0.6 g of silane coupling agent KH550.
[0077] Comparative Example 1
[0078] The difference from Example 1 is that the hydrophobic modifier in Example 1 is not added, and the mass of the base activator in the graphene oxide dispersion in Example 1 is replaced from 94 g to 104 g.
[0079] Comparative Example 2
[0080] The difference from Example 1 is that the polydimethylsiloxane emulsion is removed from the hydrophobic modifier in Example 1.
[0081] Comparative Example 3
[0082] The difference from Example 1 is that the silane coupling agent KH550 is removed from the hydrophobic modifier in Example 1.
[0083] Application Example 1
[0084] The graphene oxide and siloxane polymer composite modified geopolymer anticorrosive coating prepared in Example 1 was sprayed onto the steel bar surface. The diameter of the spray nozzle was 3 mm, the spray pressure was 4 MPa, the distance between the nozzle and the steel bar was 15 cm, the spray time was 10 s, and the spray coating amount was 0.25 g / cm 2 , and dried at 22°C for 60 min to obtain a hydrophobic geopolymer inorganic anticorrosion coating (with a thickness of 200 μm).
[0085] Application Example 2
[0086] The difference from Application Example 1 is that the graphene oxide and siloxane polymer composite modified geopolymer anti-corrosion coating prepared in Example 1 is replaced by the graphene oxide and siloxane polymer composite modified geopolymer anti-corrosion coating prepared in Example 2.
[0087] Application Example 3
[0088] The difference from Application Example 1 is that the graphene oxide and siloxane polymer composite modified geopolymer anti-corrosion coating prepared in Example 1 is replaced by the graphene oxide and siloxane polymer composite modified geopolymer anti-corrosion coating prepared in Example 3.
[0089] Comparative application example 1
[0090] The difference from Application Example 1 is that the graphene oxide and siloxane polymer composite modified geopolymer anti-corrosion coating prepared in Example 1 is replaced by the coating prepared in Comparative Example 1.
[0091] Comparative Application Example 2
[0092] The difference from Application Example 1 is that the graphene oxide and siloxane polymer composite modified geopolymer anti-corrosion coating prepared in Example 1 is replaced by the coating prepared in Comparative Example 2.
[0093] Comparative Application Example 3
[0094] The difference from Application Example 1 is that the graphene oxide and siloxane polymer composite modified geopolymer anti-corrosion coating prepared in Example 1 is replaced by the coating prepared in Comparative Example 3.
[0095] Performance Testing
[0096] (1) The contact angles of the coated steel bars prepared in Application Examples 1 to 3 and the coated steel bars prepared in Comparative Application Example 1 were tested. The contact angles were tested using a Pinzhi Chuangsi PZ-1000 large platform contact angle tester. The volume of deionized water measured each time was 3 μL. The results are shown in Table 1. Figure 1 shown.
[0097] Depend on Figure 1 It can be seen that with the increase of the amount of hydrophobic modifier, the contact angle of the coating gradually increases, and application example 1 reaches the hydrophobic stage (90-120°), and application examples 2 and 3 reach the super-hydrophobic stage (120-150°). This shows that the aluminosilicate structure of the hydrophobically modified graphene oxide-geopolymer coating is fully grafted with a large number of methyl groups, making it have good hydrophobic ability.
[0098] (2) The coated steel bars prepared in Application Examples 1 to 3, the coated steel bars prepared in Comparative Application Example 1, and the uncoated steel bars were subjected to a neutral salt spray test. The neutral salt spray was conducted by spraying a sodium chloride solution with a mass concentration of 5% on the coated steel bars in a composite salt spray test chamber. The test time was 14 days. The results are shown in Table 1. Figure 2 And as shown in Table 1.
[0099] Table 1 Mass loss rate of coated steel bars after salt spray test
[0100]
[0101] from Figure 2 As can be seen from Table 1, the results show that there is only a small amount of rust on the surface of the coated steel bars in Application Examples 1 and 2 compared with Comparative Application Example 1, and the degree of corrosion is significantly reduced. Among them, the mass loss rate of Application Example 2 is the lowest, which is reduced by 98% compared with the uncoated steel bars. This is attributed to the hydrophobicity of the coating after hydrophobic modification, which can effectively isolate the entry of chloride ions carried by water molecules, thereby preventing chloride corrosion to the steel bars. However, when the hydrophobic agent is excessively added, the coated steel bars in Application Example 3 are corroded in blocks, and the mass loss rate is close to that of Comparative Application Example 1. It shows that the corrosion resistance of Application Example 3 is reduced. This is because excessive hydrophobic groups will reduce the degree of hydration of the geopolymer, causing the high-polymerization aluminosilicate structure to be transformed into a low-polymerization structure, weakening the density of the graphene oxide-geopolymer coating, thereby causing local corrosion of the coated steel bars.
[0102] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention rather than all the embodiments. People can also obtain other embodiments based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.
Claims
1. A graphene oxide and siloxane polymer composite modified geopolymer anticorrosion coating, characterized in that: The raw materials for preparation include the following components by weight:
2. The graphene oxide and siloxane polymer composite modified geopolymer anticorrosion coating according to claim 1, characterized in that: The specific surface area of the graphene oxide is 100 to 400 m 2 / g; the number of layers of the graphene oxide is 1 to 2 layers; and the sheet diameter of the graphene oxide is 0.2 to 10 μm.
3. The graphene oxide and siloxane polymer composite modified geopolymer anticorrosion coating according to claim 1, characterized in that: The silicone polymer is polydimethylsiloxane.
4. The graphene oxide and siloxane polymer composite modified geopolymer anticorrosion coating according to claim 1, characterized in that: The silane coupling agent is silane coupling agent KH550.
5. The graphene oxide and siloxane polymer composite modified geopolymer anticorrosive coating according to claim 1, characterized in that: The alkaline activator comprises sodium hydroxide, water and water glass; the modulus of the alkaline activator is 1.3-2M.
6. The graphene oxide and siloxane polymer composite modified geopolymer anticorrosive coating according to claim 1, characterized in that: The aluminosilicate minerals include one or more of fly ash, slag and metakaolin.
7. The method for preparing the graphene oxide and siloxane polymer composite modified geopolymer anticorrosion coating according to any one of claims 1 to 6, characterized in that: The following steps are involved: first mixing a portion of the alkaline activator, graphene oxide and a surfactant to obtain a graphene oxide dispersion; The siloxane polymer, the silane coupling agent and the remaining base activator are mixed and hydrolyzed to obtain a hydrophobic modifier; The graphene oxide dispersion, the organosilicon defoamer, the hydrophobic modifier, the aluminosilicate mineral, the polyvinyl alcohol powder and the titanium dioxide are thirdly mixed to obtain a graphene oxide and siloxane polymer composite modified geopolymer anticorrosive coating.
8. Use of the graphene oxide and siloxane polymer composite modified geopolymer anti-corrosion coating according to any one of claims 1 to 6 or the graphene oxide and siloxane polymer composite modified geopolymer anti-corrosion coating prepared by the preparation method according to claim 7 in steel corrosion protection.
9. A method for preparing a hydrophobic geopolymer inorganic anticorrosive coating, characterized in that: The following steps are involved: The graphene oxide and siloxane polymer composite modified geopolymer anti-corrosion coating is applied on the surface of steel and dried to obtain a hydrophobic geopolymer inorganic anti-corrosion coating; The graphene oxide and siloxane polymer composite modified geopolymer anti-corrosion coating is the graphene oxide and siloxane polymer composite modified geopolymer anti-corrosion coating according to any one of claims 1 to 6 or the graphene oxide and siloxane polymer composite modified geopolymer anti-corrosion coating prepared by the preparation method according to claim 7.
10. The preparation method according to claim 9, characterized in that: The coating is spraying; the diameter of the spraying nozzle is 2-4 mm; the spraying pressure is 3-5 MPa; the distance between the spraying nozzle and the steel is 12-18 cm; the spraying time is 10-15 s; the spraying coating amount is 0.2-0.3 g / cm 2 .
Citation Information
Patent Citations
Hydrophobic antibacterial geopolymer material for marine concrete structure and preparation method thereof
CN110981297A
Super-hydrophobic geopolymer prepared by microcellular foaming and preparation method thereof
CN112079585A
Siloxane-modified super-hydrophobic geopolymer anticorrosive material and preparation method thereof
CN112079593A
Geopolymer coating as well as preparation method and application thereof
CN118240403A
Coating compositions for hydrophobic films and articles having hydrophobic surfaces
US20220363919A1
Cited By
Fireproof and flame-retardant integrated coating and preparation method thereof
CN119432228A
High-temperature-resistant inorganic coating prepared from metallurgical solid waste, preparation method and application of high-temperature-resistant inorganic coating, and composite structure
CN119859050A