Composite powder suitable for environment-friendly coating and method for preparing environment-friendly coating by using composite powder

By using composite powders prepared by wollastonite and other materials, the hazards of organic solvents in traditional coatings and the complex and high cost of composite powders are solved, and the preparation of high-performance environmentally friendly coatings is realized, meeting environmental protection and performance needs.

CN118909479APending Publication Date: 2024-11-08JIANGXI GUANGYUAN CHEM +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411155272.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The use of organic solvents in traditional coatings leads to environmental and human health hazards, and the existing composite powders are complex in the preparation process, high cost and unstable in performance, making it difficult to meet the needs of environmentally friendly coatings.

Method used

A composite powder composed of wollastonite, magnesium hydroxide, silicon micropowder, barium sulfate, talc powder and calcium carbonate was prepared by ball milling, drying and screening treatment, and Mix it with water-based resin and other materials to prepare environmentally friendly coatings.

Benefits of technology

Improve the coating's hiding power, weather resistance and corrosion resistance, simplify the preparation process, reduce energy consumption and production costs, improve dispersion and compatibility, meet the market's demand for high-performance environmentally friendly coatings, and reduce VOCs emission.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of composite powder, in particular to composite powder suitable for an environment-friendly coating and a method for preparing the environment-friendly coating from the composite powder. The composite powder is prepared from the following raw materials in parts by weight: 20-30 parts of wollastonite, 15-25 parts of magnesium hydroxide, 10-20 parts of silica powder, 5-15 parts of barium sulfate, 10-20 parts of talcum powder and 5-15 parts of calcium carbonate, and the preparation method comprises the following steps: firstly, weighing the raw materials in parts by weight and uniformly mixing to form a mixture; putting the mixture into a ball mill for grinding treatment; carrying out drying treatment on the ground mixture; and screening the dried mixture to obtain the finished product composite powder. The invention provides composite powder suitable for an environment-friendly coating and a method for preparing the environment-friendly coating from the composite powder, the composite powder is composed of wollastonite, magnesium hydroxide, silica powder, barium sulfate, talcum powder, calcium carbonate and other raw materials, and the environment-friendly coating with high purity and stability can be prepared.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of composite powders, and in particular to a composite powder suitable for environmentally friendly coatings and a method for preparing environmentally friendly coatings using the composite powders. Background Art

[0002] In the coatings industry, the demand for environmentally friendly coatings is growing, mainly due to the increasing awareness of health and environmental protection. Traditional coating products often contain a large amount of organic solvents, which release volatile organic compounds (VOCs) during the production and use of coatings, causing harm to the environment and human health.

[0003] Although the application of traditional inorganic fillers in coatings can reduce the content of VOC, they often have problems such as poor dispersibility and poor compatibility with resins, resulting in unsatisfactory physical properties and decorative effects of the coatings. In order to solve these problems, researchers began to explore the use of composite powders as fillers in coatings in order to obtain better performance.

[0004] Composite powder is a mixture of multiple inorganic materials in a specific ratio. It can combine the advantages of various materials, such as improving the hiding power, weather resistance, corrosion resistance, etc. of the coating. At the same time, the particle size distribution and surface characteristics of the composite powder can be precisely controlled, thereby improving its dispersibility in the coating and its compatibility with the resin.

[0005] In the existing technology, although some composite powders have been used in the preparation of environmentally friendly coatings, these composite powders often have problems such as complex preparation process, high cost, unstable performance, etc. For example, some composite powders require high-temperature sintering during the preparation process, which not only increases energy consumption but also may introduce new pollution problems. In addition, due to the different thermal expansion coefficients of different inorganic materials, high-temperature treatment may cause stress inside the composite powder, affecting its application performance in the coating. Summary of the invention

[0006] The present invention proposes a composite powder suitable for environmentally friendly coatings and a method for preparing environmentally friendly coatings using the composite powder. The composite powder is composed of raw materials such as wollastonite, magnesium hydroxide, silicon micropowder, barium sulfate, talcum powder and calcium carbonate, and can be used to prepare environmentally friendly coatings with high purity and stability.

[0007] The technical solution adopted by the present invention is: a composite powder suitable for environmentally friendly coatings, the composite powder is composed of the following raw materials in parts by weight: wollastonite accounts for 20-30 parts, magnesium hydroxide accounts for 15-25 parts, silicon micropowder accounts for 10-20 parts, barium sulfate accounts for 5-15 parts, talc accounts for 10-20 parts, and calcium carbonate accounts for 5-15 parts.

[0008] The preparation method of the composite powder comprises the following steps:

[0009] Step 1: First, weigh wollastonite, magnesium hydroxide, silicon powder, barium sulfate, talc, and calcium carbonate according to the above weight proportions, and mix them evenly to form a mixture;

[0010] Step 2: Put the mixture into a ball mill for grinding to ensure that the raw materials are fully refined;

[0011] Step 3: Drying the ground mixture to remove moisture from the mixture;

[0012] Step 4: Screening the dried mixture to obtain finished composite powder.

[0013] As a further improvement of the present invention, the grinding treatment time is 2-4 hours; the drying treatment temperature is controlled at 80-100°C, and the drying treatment time is 60-90 minutes; the screening treatment is carried out using a standard sieve with a mesh size of 80-120.

[0014] A method for preparing an environmentally friendly coating using composite powders comprises the following steps:

[0015] S1: Weigh 20 parts of composite powder, 40 parts of water-based resin, 2 parts of dispersant, 1 part of defoamer, 1 part of preservative, 2 parts of thickener, 8 parts of pigment, and 40 parts of deionized water by weight;

[0016] S2: Mix and stir the water-based resin, dispersant, defoamer, preservative, thickener, pigment and 1 / 2 of deionized water to form a base liquid;

[0017] S3: adding the composite powder and the remaining 1 / 2 of deionized water to the base liquid, mixing and stirring to obtain a mixed solution;

[0018] S4: filtering the obtained mixed solution to remove impurities and particles therein to obtain a coating with high purity and stability;

[0019] S5: homogenize the filtered paint to obtain a finished environmentally friendly paint.

[0020] As a further improvement of the present invention, in S1, the water-based resin includes one or more of water-based fluororesin, water-based polyurethane resin, and water-based acrylic resin;

[0021] The dispersant includes one of ammonium polymethacrylate and octadeceneamine acetate;

[0022] The defoaming agent includes one of polydimethylsiloxane and polypropylene glycol;

[0023] The preservative includes one of methyl paraben, propylene glycol, and methyl benzoate;

[0024] The thickener includes one of hydroxyethyl cellulose, methyl cellulose, bentonite and magnesium aluminum silicate.

[0025] As a further improvement of the present invention, in S2, the mixing speed is controlled at 140-180 rpm, and the mixing time is controlled at 20-30 minutes.

[0026] As a further improvement of the present invention, in S3, the mixing speed is controlled at 150-200 rpm, and the mixing time is controlled at 40-60 minutes.

[0027] As a further improvement of the present invention, in S4, the medium for filtering treatment is a filter cloth with a mesh size of 120 or more.

[0028] As a further improvement of the present invention, in S5, the pressure of the homogenization treatment is controlled at 50-100 MPa, the number of homogenizations is 2-4 times, and the interval time of each time is controlled at 5-10 minutes.

[0029] The beneficial effects of the present invention are as follows: (1) The present invention adopts raw materials such as wollastonite, magnesium hydroxide, silicon micropowder, barium sulfate, talcum powder and calcium carbonate, which can effectively improve the hiding power, weather resistance, corrosion resistance and other properties of the coating, while maintaining the environmental protection characteristics of the coating and reducing the emission of VOCs.

[0030] (2) The composite powder preparation method of the present invention is simple and avoids high-energy consumption and potentially polluting processes such as high-temperature sintering, thereby reducing production costs while ensuring stable performance of the composite powder.

[0031] (3) The present invention ensures that the particle size distribution and surface characteristics of the composite powder are precisely controlled by optimizing the mixing, grinding, drying and screening steps, thereby improving its dispersibility in the coating and its compatibility with the resin, and improving the physical properties and decorative effects of the coating.

[0032] (4) The environmentally friendly coating prepared by the present invention using composite powder has a simple preparation process, low cost, and high purity and stability of the coating, thus meeting the market demand for high-performance environmentally friendly coatings.

[0033] (5) The environmentally friendly coating prepared by the composite powder of the present invention contains no or very low amounts of organic solvents, is environmentally friendly, harmless to human health, and complies with the current development trend of the coating industry and environmental protection requirements. DETAILED DESCRIPTION

[0034] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present application more clearly understood, the present application is further described in detail below in conjunction with the embodiments. It should be understood that the embodiments described herein are only used to explain the present application and are not used to limit the present application.

[0035] The present invention provides a composite powder suitable for environmentally friendly coatings. The composite powder is composed of the following raw materials in parts by weight: 20-30 parts of wollastonite, 15-25 parts of magnesium hydroxide, 10-20 parts of silicon micropowder, 5-15 parts of barium sulfate, 10-20 parts of talc, and 5-15 parts of calcium carbonate.

[0036] The preparation method of the composite powder comprises the following steps: firstly, wollastonite, magnesium hydroxide, silicon powder, barium sulfate, talcum powder and calcium carbonate are weighed according to the above-mentioned weight proportions, and mixed evenly to form a mixture; the mixture is put into a ball mill for grinding to ensure that the raw materials are fully refined; the ground mixture is dried to remove moisture from the mixture; the dried mixture is sieved to obtain a finished composite powder.

[0037] The grinding time of the present invention is 2-4 hours; the drying temperature is controlled at 80-100°C, and the drying time is 60-90 minutes; the screening process is carried out using a standard screen with a mesh size of 80-120.

[0038] A method for preparing an environmentally friendly coating using composite powders comprises the following steps: weighing 20 parts of composite powders and 40 parts of water-based resin, 2 parts of dispersant, 1 part of defoamer, 1 part of preservative, 2 parts of thickener, 8 parts of pigment, and 40 parts of deionized water by weight; mixing and stirring the water-based resin, dispersant, defoamer, preservative, thickener, pigment, and 1 / 2 of deionized water to form a base liquid; adding the composite powder and the remaining 1 / 2 of deionized water to the base liquid, mixing and stirring, and obtaining a mixed solution; filtering the obtained mixed solution to remove impurities and particles therein, and obtaining a coating with high purity and stability; and homogenizing the filtered coating to obtain a finished environmentally friendly coating.

[0039] In S1 of the present invention, the water-based resin includes one or more of water-based fluororesin, water-based polyurethane resin, and water-based acrylic resin; the dispersant includes one of ammonium polymethacrylate and octadecylamine acetate; the defoamer includes one of polydimethylsiloxane and polypropylene glycol; the preservative includes one of methyl parahydroxybenzoate, propylene glycol, and methyl benzoate; the thickener includes one of hydroxyethyl cellulose, methyl cellulose, bentonite, and magnesium aluminum silicate.

[0040] In S2 of the present invention, the mixing speed is controlled at 140-180 rpm, and the mixing time is controlled at 20-30 minutes.

[0041] In S3 of the present invention, the mixing speed is controlled at 150-200 rpm, and the mixing time is controlled at 40-60 minutes.

[0042] In S4 of the present invention, the medium for filtration treatment is a filter cloth having a mesh size of 120 or more.

[0043] In S5 of the present invention, the pressure of the homogenization treatment is controlled at 50-100 MPa, the number of homogenizations is 2-4 times, and the interval time between each times is controlled at 5-10 minutes.

[0044] Embodiment 1:

[0045] This embodiment provides a composite powder suitable for environmentally friendly coatings and a method for preparing environmentally friendly coatings using the composite powder, which specifically includes the following steps.

[0046] (i) Weigh 25 parts of wollastonite, 20 parts of magnesium hydroxide, 15 parts of silica powder, 10 parts of barium sulfate, 15 parts of talc powder, and 10 parts of calcium carbonate by weight, and mix them evenly to form a mixture;

[0047] (ii) grinding the mixture in a ball mill for 3 hours to ensure that the raw materials are fully refined;

[0048] (3) drying the ground mixture at a temperature of 90° C. for 80 minutes to remove moisture from the mixture;

[0049] (iv) using a standard sieve with a mesh size of 100 to sieve the dried mixture to obtain a finished composite powder.

[0050] (V) Weigh 20 parts of the composite powder obtained above, 40 parts of water-based fluororesin, 2 parts of ammonium polymethacrylate, 1 part of polydimethylsiloxane, 1 part of methylparaben, 2 parts of hydroxyethylcellulose, 8 parts of pigment, and 40 parts of deionized water by weight;

[0051] (vi) mixing and stirring the water-based fluororesin, ammonium polymethacrylate, polydimethylsiloxane, methyl paraben, hydroxyethyl cellulose, pigment and 1 / 2 of deionized water at a mixing speed of 160 rpm for 25 minutes to form a base liquid;

[0052] (VII) adding the composite powder and the remaining 1 / 2 of deionized water to the base liquid, mixing and stirring, wherein the mixing and stirring speed is controlled at 180 rpm, and the mixing and stirring time is controlled at 50 minutes to obtain a mixed solution;

[0053] (VIII) filtering the obtained mixed solution with a 150-mesh filter cloth to remove impurities and particles therein to obtain a coating with high purity and stability;

[0054] (IX) The filtered coating is homogenized, wherein the pressure of the homogenization is controlled at 80 MPa, the number of homogenizations is 3, and the interval time between each homogenization is controlled at 8 minutes, to obtain a finished environmentally friendly coating.

[0055] Embodiment 2:

[0056] This embodiment provides a composite powder suitable for environmentally friendly coatings and a method for preparing environmentally friendly coatings using the composite powder, which specifically includes the following steps.

[0057] (i) Weigh 25 parts of wollastonite, 24 parts of magnesium hydroxide, 18 parts of silica powder, 12 parts of barium sulfate, 18 parts of talc powder, and 12 parts of calcium carbonate by weight, and mix them evenly to form a mixture;

[0058] (ii) grinding the mixture in a ball mill for 3.5 hours to ensure that the raw materials are fully refined;

[0059] (3) drying the ground mixture at a temperature of 95° C. for 80 minutes to remove moisture from the mixture;

[0060] (iv) using a standard sieve with a mesh size of 110 to sieve the dried mixture to obtain a finished composite powder.

[0061] (V) Weigh 20 parts of the composite powder obtained above, 40 parts of water-based fluororesin, 2 parts of ammonium polymethacrylate, 1 part of polydimethylsiloxane, 1 part of methylparaben, 2 parts of hydroxyethylcellulose, 8 parts of pigment, and 40 parts of deionized water by weight;

[0062] (vi) mixing and stirring the water-based fluororesin, ammonium polymethacrylate, polydimethylsiloxane, methyl paraben, hydroxyethyl cellulose, pigment and 1 / 2 of deionized water at a mixing speed of 160 rpm for 25 minutes to form a base liquid;

[0063] (VII) adding the composite powder and the remaining 1 / 2 of deionized water to the base liquid, mixing and stirring, wherein the mixing and stirring speed is controlled at 180 rpm, and the mixing and stirring time is controlled at 50 minutes to obtain a mixed solution;

[0064] (VIII) filtering the obtained mixed solution with a 150-mesh filter cloth to remove impurities and particles therein to obtain a coating with high purity and stability;

[0065] (IX) The filtered coating is homogenized, wherein the pressure of the homogenization is controlled at 80 MPa, the number of homogenizations is 3, and the interval time between each homogenization is controlled at 8 minutes, to obtain a finished environmentally friendly coating.

[0066] Embodiment 3:

[0067] This embodiment provides a composite powder suitable for environmentally friendly coatings and a method for preparing environmentally friendly coatings using the composite powder, which specifically includes the following steps.

[0068] (i) Weigh 24 parts of wollastonite, 18 parts of magnesium hydroxide, 12 parts of silicon powder, 8 parts of barium sulfate, 12 parts of talc, and 8 parts of calcium carbonate by weight, and mix them evenly to form a mixture;

[0069] (ii) grinding the mixture in a ball mill for 2.5 hours to ensure that the raw materials are fully refined;

[0070] (iii) drying the ground mixture at a temperature of 85° C. for 70 minutes to remove moisture from the mixture;

[0071] (iv) using a standard sieve with a mesh size of 100 to sieve the dried mixture to obtain a finished composite powder.

[0072] (V) Weigh 20 parts of the composite powder obtained above, 40 parts of water-based fluororesin, 2 parts of ammonium polymethacrylate, 1 part of polydimethylsiloxane, 1 part of methylparaben, 2 parts of hydroxyethylcellulose, 8 parts of pigment, and 40 parts of deionized water by weight;

[0073] (vi) mixing and stirring the water-based fluororesin, ammonium polymethacrylate, polydimethylsiloxane, methyl paraben, hydroxyethyl cellulose, pigment and 1 / 2 of deionized water at a mixing speed of 160 rpm for 25 minutes to form a base liquid;

[0074] (VII) adding the composite powder and the remaining 1 / 2 of deionized water to the base liquid, mixing and stirring, wherein the mixing and stirring speed is controlled at 180 rpm, and the mixing and stirring time is controlled at 50 minutes to obtain a mixed solution;

[0075] (VIII) filtering the obtained mixed solution with a 150-mesh filter cloth to remove impurities and particles therein to obtain a coating with high purity and stability;

[0076] (IX) The filtered coating is homogenized, wherein the pressure of the homogenization is controlled at 80 MPa, the number of homogenizations is 3, and the interval time between each homogenization is controlled at 8 minutes, to obtain a finished environmentally friendly coating.

[0077] Embodiment 4:

[0078] This embodiment provides a composite powder suitable for environmentally friendly coatings and a method for preparing environmentally friendly coatings using the composite powder, which specifically includes the following steps.

[0079] (i) Weigh 25 parts of wollastonite, 20 parts of magnesium hydroxide, 15 parts of silica powder, 10 parts of barium sulfate, 15 parts of talc powder, and 10 parts of calcium carbonate by weight, and mix them evenly to form a mixture;

[0080] (ii) grinding the mixture in a ball mill for 3 hours to ensure that the raw materials are fully refined;

[0081] (3) drying the ground mixture at a temperature of 90° C. for 80 minutes to remove moisture from the mixture;

[0082] (iv) using a standard sieve with a mesh size of 100 to sieve the dried mixture to obtain a finished composite powder.

[0083] (V) Weighing 20 parts of the composite powder obtained above, 40 parts of waterborne polyurethane resin, 2 parts of ammonium polymethacrylate, 1 part of polypropylene glycol, 1 part of methyl benzoate, 2 parts of hydroxyethyl cellulose, 8 parts of pigment, and 40 parts of deionized water by weight;

[0084] (vi) mixing and stirring the waterborne polyurethane resin, ammonium polymethacrylate, polypropylene glycol, methyl benzoate, hydroxyethyl cellulose, pigment and 1 / 2 of deionized water at a mixing speed of 160 rpm for 25 minutes to form a base liquid;

[0085] (VII) adding the composite powder and the remaining 1 / 2 of deionized water to the base liquid, mixing and stirring, wherein the mixing and stirring speed is controlled at 180 rpm, and the mixing and stirring time is controlled at 50 minutes to obtain a mixed solution;

[0086] (VIII) filtering the obtained mixed solution with a 150-mesh filter cloth to remove impurities and particles therein to obtain a coating with high purity and stability;

[0087] (IX) The filtered coating is homogenized, wherein the pressure of the homogenization is controlled at 80 MPa, the number of homogenizations is 3, and the interval time between each homogenization is controlled at 8 minutes, to obtain a finished environmentally friendly coating.

[0088] Embodiment 5:

[0089] This embodiment provides a composite powder suitable for environmentally friendly coatings and a method for preparing environmentally friendly coatings using the composite powder, which specifically includes the following steps.

[0090] (i) Weigh 25 parts of wollastonite, 20 parts of magnesium hydroxide, 15 parts of silica powder, 10 parts of barium sulfate, 15 parts of talc powder, and 10 parts of calcium carbonate by weight, and mix them evenly to form a mixture;

[0091] (ii) grinding the mixture in a ball mill for 3 hours to ensure that the raw materials are fully refined;

[0092] (3) drying the ground mixture at a temperature of 90° C. for 80 minutes to remove moisture from the mixture;

[0093] (iv) using a standard sieve with a mesh size of 100 to sieve the dried mixture to obtain a finished composite powder.

[0094] (V) Weigh 20 parts of the composite powder obtained above, 20 parts of water-based fluororesin and 20 parts of water-based acrylic resin, 2 parts of octadecylamine acetate, 1 part of polydimethylsiloxane, 1 part of methyl paraben, 2 parts of magnesium aluminum silicate, 8 parts of pigment, and 40 parts of deionized water by weight;

[0095] (vi) mixing and stirring the water-based fluororesin and water-based acrylic resin, octadecylamine acetate, polydimethylsiloxane, methylparaben, magnesium aluminum silicate, pigment and 1 / 2 of deionized water at a mixing speed of 160 rpm for 25 minutes to form a base liquid;

[0096] (VII) adding the composite powder and the remaining 1 / 2 of deionized water to the base liquid, mixing and stirring, wherein the mixing and stirring speed is controlled at 180 rpm, and the mixing and stirring time is controlled at 50 minutes to obtain a mixed solution;

[0097] (VIII) filtering the obtained mixed solution with a 150-mesh filter cloth to remove impurities and particles therein to obtain a coating with high purity and stability;

[0098] (IX) The filtered coating is homogenized, wherein the pressure of the homogenization is controlled at 80 MPa, the number of homogenizations is 3, and the interval time between each homogenization is controlled at 8 minutes, to obtain a finished environmentally friendly coating.

[0099] Embodiment 6:

[0100] This embodiment provides a composite powder suitable for environmentally friendly coatings and a method for preparing environmentally friendly coatings using the composite powder, which specifically includes the following steps.

[0101] (i) Weigh 25 parts of wollastonite, 20 parts of magnesium hydroxide, 15 parts of silica powder, 10 parts of barium sulfate, 15 parts of talc powder, and 10 parts of calcium carbonate by weight, and mix them evenly to form a mixture;

[0102] (ii) grinding the mixture in a ball mill for 3 hours to ensure that the raw materials are fully refined;

[0103] (3) drying the ground mixture at a temperature of 90° C. for 80 minutes to remove moisture from the mixture;

[0104] (iv) using a standard sieve with a mesh size of 100 to sieve the dried mixture to obtain a finished composite powder.

[0105] (V) Weigh 20 parts of the composite powder obtained above, 40 parts of water-based fluororesin, 2 parts of ammonium polymethacrylate, 1 part of polydimethylsiloxane, 1 part of methylparaben, 2 parts of hydroxyethylcellulose, 8 parts of pigment, and 40 parts of deionized water by weight;

[0106] (vi) mixing and stirring the water-based fluororesin, ammonium polymethacrylate, polydimethylsiloxane, methyl paraben, hydroxyethyl cellulose, pigment and 1 / 2 of deionized water at a mixing speed of 150 rpm for 28 minutes to form a base liquid;

[0107] (VII) adding the composite powder and the remaining 1 / 2 of deionized water to the base liquid, mixing and stirring, wherein the mixing and stirring speed is controlled at 180 rpm, and the mixing and stirring time is controlled at 55 minutes to obtain a mixed solution;

[0108] (VIII) filtering the obtained mixed solution with a 150-mesh filter cloth to remove impurities and particles therein to obtain a coating with high purity and stability;

[0109] (IX) The filtered coating is homogenized, wherein the pressure of the homogenization is controlled at 70 MPa, the number of homogenizations is 3, and the interval time of each homogenization is controlled at 7 minutes, to obtain a finished environmentally friendly coating.

[0110] Embodiment 7:

[0111] This embodiment provides a composite powder suitable for environmentally friendly coatings and a method for preparing environmentally friendly coatings using the composite powder, which specifically includes the following steps.

[0112] (i) Weigh 25 parts of wollastonite, 24 parts of magnesium hydroxide, 18 parts of silica powder, 12 parts of barium sulfate, 18 parts of talc powder, and 12 parts of calcium carbonate by weight, and mix them evenly to form a mixture;

[0113] (ii) grinding the mixture in a ball mill for 3.5 hours to ensure that the raw materials are fully refined;

[0114] (3) drying the ground mixture at a temperature of 95° C. for 80 minutes to remove moisture from the mixture;

[0115] (iv) using a standard sieve with a mesh size of 100 to sieve the dried mixture to obtain a finished composite powder.

[0116] (V) Weigh 20 parts of the composite powder obtained above, 40 parts of water-based fluororesin, 2 parts of ammonium polymethacrylate, 1 part of polydimethylsiloxane, 1 part of methylparaben, 2 parts of hydroxyethylcellulose, 8 parts of pigment, and 40 parts of deionized water by weight;

[0117] (vi) mixing and stirring the water-based fluororesin, ammonium polymethacrylate, polydimethylsiloxane, methyl paraben, hydroxyethyl cellulose, pigment and 1 / 2 of deionized water at a mixing speed of 150 rpm for 28 minutes to form a base liquid;

[0118] (VII) adding the composite powder and the remaining 1 / 2 of deionized water to the base liquid, mixing and stirring, wherein the mixing and stirring speed is controlled at 180 rpm, and the mixing and stirring time is controlled at 55 minutes to obtain a mixed solution;

[0119] (VIII) filtering the obtained mixed solution with a 150-mesh filter cloth to remove impurities and particles therein to obtain a coating with high purity and stability;

[0120] (IX) The filtered coating is homogenized, wherein the pressure of the homogenization is controlled at 70 MPa, the number of homogenizations is 3, and the interval time of each homogenization is controlled at 7 minutes, to obtain a finished environmentally friendly coating.

[0121] Performance Testing

[0122] The environmentally friendly coatings obtained in the above Examples 1-7 were subjected to performance tests, and common coatings on the market were used as comparative examples.

[0123] Test items include: Adhesion (test standard: GB / T9286-1998); Hardness (test standard: GB / T6739-2006); Soluble aluminum (test standard: EN71-3); Alcohol resistance (test standard: GB / T23989-2009); Adhesion resistance (test standard: GB / T1762-1980); Scratch resistance (test standard: GB / T9279-2007); Storage stability (test standard: GB / T6753.3-1986)

[0124] sample Adhesion hardness Soluble aluminum Alcohol resistance Back adhesion Scratch resistance Storage stability Example 1 Level 0 2H qualified 600 times Level 1 620g excellent Example 2 Level 0 2H qualified 580 times Level 1 600g excellent Example 3 Level 0 2H qualified 610 times Level 1 610g excellent Example 4 Level 0 2H qualified 580 times Level 1 620g excellent Example 5 Level 0 2H qualified 590 times Level 1 610g excellent Example 6 Level 0 2H qualified 600 times Level 1 630g excellent Example 7 Level 0 2H qualified 610 times Level 1 620g excellent Comparative Example Level 0 H Failure 200 times Level 2 400g Difference

[0125] As can be seen from the above table, the environmentally friendly coatings of Examples 1 to 7 all performed well in various performance tests, and were significantly better than the common coatings on the market. Specifically, the coatings of Examples 1 to 7 all reached level 0 in the adhesion test, indicating that they had excellent adhesion to the substrate; they all reached 2H in the hardness test, which was much higher than the level H of the comparative example, indicating that they had high surface hardness and good wear resistance; they all passed the soluble aluminum test, while the comparative example failed, indicating that the coatings of the embodiments were better in terms of safety; in the alcohol resistance test, the coatings of the embodiments all exceeded 580 times, which was much higher than the 200 times of the comparative example, indicating that they had excellent solvent resistance; in the re-adhesion test, the coatings of the embodiments were all at level 1, while the comparative example was at level 2, indicating that the coatings of the embodiments were not easy to re-adhere and had better performance; in the scratch resistance test, the coatings of the embodiments were all above 600g, which was much higher than the 400g of the comparative example, indicating that they had excellent scratch resistance; in the storage stability test, the coatings of the embodiments were all rated as excellent, while the comparative example was rated as poor, indicating that the coatings of the embodiments had good stability during storage and were not easy to deteriorate.

[0126] In summary, the environmentally friendly coating prepared using the composite powder of the present invention performs well in various performance indicators and has significant market application value and promotion prospects; its excellent performance not only meets the health and safety requirements of modern environmentally friendly coatings, but also shows excellent durability and practicality in practical applications.

[0127] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features thereof may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A composite powder suitable for environmentally friendly coatings, characterized in that: The composite powder is composed of the following raw materials in parts by weight: wollastonite accounts for 20-30 parts, magnesium hydroxide accounts for 15-25 parts, silicon micropowder accounts for 10-20 parts, barium sulfate accounts for 5-15 parts, talc accounts for 10-20 parts, and calcium carbonate accounts for 5-15 parts. The preparation method of the composite powder comprises the following steps: Step 1: First, weigh wollastonite, magnesium hydroxide, silicon powder, barium sulfate, talc, and calcium carbonate according to the above weight proportions, and mix them evenly to form a mixture; Step 2: Put the mixture into a ball mill for grinding to ensure that the raw materials are fully refined; Step 3: Drying the ground mixture to remove moisture from the mixture; Step 4: Screening the dried mixture to obtain finished composite powder.

2. The composite powder suitable for environmentally friendly coatings according to claim 1, characterized in that: The grinding treatment takes 2-4 hours; the drying treatment temperature is controlled at 80-100°C, and the drying treatment time is 60-90 minutes; the screening treatment is performed using a standard screen with a mesh size of 80-120.

3. A method for preparing an environmentally friendly coating using composite powder, characterized in that: The steps include: S1: Weigh 20 parts of composite powder, 40 parts of water-based resin, 2 parts of dispersant, 1 part of defoamer, 1 part of preservative, 2 parts of thickener, 8 parts of pigment, and 40 parts of deionized water by weight; S2: Mix and stir the water-based resin, dispersant, defoamer, preservative, thickener, pigment and 1 / 2 of deionized water to form a base liquid; S3: adding the composite powder and the remaining 1 / 2 of deionized water to the base liquid, mixing and stirring to obtain a mixed solution; S4: filtering the obtained mixed solution to remove impurities and particles therein to obtain a coating with high purity and stability; S5: homogenize the filtered paint to obtain a finished environmentally friendly paint.

4. The method for preparing an environmentally friendly coating using composite powder according to claim 3, characterized in that: In S1, the water-based resin includes one or more of water-based fluororesin, water-based polyurethane resin, and water-based acrylic resin; The dispersant includes one of ammonium polymethacrylate and octadeceneamine acetate; The defoaming agent includes one of polydimethylsiloxane and polypropylene glycol; The preservative includes one of methyl paraben, propylene glycol, and methyl benzoate; The thickener includes one of hydroxyethyl cellulose, methyl cellulose, bentonite and magnesium aluminum silicate.

5. The method for preparing environmentally friendly coatings using composite powders according to claim 3, characterized in that: In S2, the mixing speed is controlled at 140-180 rpm, and the mixing time is controlled at 20-30 minutes.

6. The method for preparing an environmentally friendly coating using composite powder according to claim 3, characterized in that: In S3, the mixing speed is controlled at 150-200 rpm, and the mixing time is controlled at 40-60 minutes.

7. The method for preparing environmentally friendly coatings using composite powders according to claim 3, characterized in that: In the above S4, the medium for the filtration treatment is a filter cloth having a mesh size of 120 or more.

8. The method for preparing environmentally friendly coatings using composite powders according to claim 3, characterized in that: In S5, the pressure of the homogenization treatment is controlled at 50-100 MPa, the number of homogenizations is 2-4 times, and the interval time between each time is controlled at 5-10 minutes.

Citation Information

Patent Citations

  • Concrete bridge structure surface protective coating material based on pure acrylic emulsion and preparation method thereof

    CN103045041A

  • Mildew-proof and water-resistant putty powder for inner wall

    CN106084972A

  • High-hardness coating for shell of aluminum charger and preparation method thereof

    CN106675231A

  • Composite filler for water-based paint and preparation method of composite filler

    CN112852212A

  • Aqueous resin dispersion and water-based coating composition for inorganic building material

    JP2002145969A