Green curing high-weather-resistance self-repairing polyurethane waterproof coating as well as preparation method and application thereof

By using aliphatic isocyanate and small molecule self-healing chain extender in polyurethane waterproof coatings, combined with ultraviolet absorbers and light stabilizers, the chemical hazards, weather-to-weather and oxygen-tolerant problems of polyurethane waterproof coatings are solved, and high weather resistance and Self-healing ability improves the mechanical properties and service life of the coating.

CN118931355APending Publication Date: 2024-11-12JIANGSU BOLIKANG NEW MATERIAL TECHNOLOGY CO LTD +1

Patent Information

Application Number
CN202411195350.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Existing polyurethane waterproof coatings have problems such as high chemical harm, weather resistance, oxygen resistance, and inability to heal, which limits their application range and lifespan.

Method used

Use aliphatic isocyanate as raw material to adjust the isocyanate content, and add small molecule self-healing chain extender and hydrophilic chain extender, combine benzotriazole ultraviolet absorbers and hindered amine light stabilizers to improve coating through green curing Tensile strength and self-healing ability of the layer.

Benefits of technology

It realizes the high weather resistance, oxygen resistance and self-healing ability of polyurethane waterproof coatings, improves the mechanical properties and service life of the coating, and has a simple process, low cost, environmental protection and pollution-free.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118931355A_ABST
    Figure CN118931355A_ABST
Patent Text Reader

Abstract

The invention provides a green curing high-weather-resistance self-repairing polyurethane waterproof coating as well as a preparation method and application thereof. The waterproof coating is prepared from the following raw materials: a polyol oligomer, diisocyanate, a hydrophilic chain extender, a self-repairing micromolecule chain extender, a weather-resistant and oxygen-resistant aid, nano titanium dioxide and a catalyst. The coating further comprises the following raw materials: an inorganic powder filler, a gas absorbent, a liquid filler, a wetting dispersant, a defoaming agent and an anti-settling agent. Aliphatic isocyanate or alicyclic isocyanate with excellent weather resistance and yellowing resistance is adopted as a base material, and the ageing resistance of the polyurethane waterproof coating is improved by adding the nano titanium dioxide and the weather-resistant and oxygen-resistant additive; a reversible recombination self-repairing group is introduced in the synthesis process of the polyurethane prepolymer; polyurethane chain extension is completed in a green curing manner, so that the mechanical strength of the coating is improved, and the environment friendliness of the waterproof coating is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of coating preparation, and in particular to a method for preparing a green-curing, highly weather-resistant and self-repairing polyurethane waterproof coating. Background Art

[0002] Polyurethane waterproof coatings have the advantages of high strength, good elasticity, strong adhesion, good wear resistance, high and low temperature resistance, corrosion resistance and convenient construction. With the progress of science and technology and the development of chemical building materials industry in my country, polyurethane waterproof coatings have also been developed. Due to the adjustability of polyurethane molecular chains and mature preparation and production processes, polyurethane waterproof coatings with different functions can be produced according to the requirements of different waterproof engineering projects.

[0003] Toluene diisocyanate (TDI) and diphenylmethane diisocyanate (MDI) are cheap and have excellent performance, so they are widely used as raw materials for polyurethane waterproof coatings. However, the methyl groups on the benzene rings of these two raw materials will oxidize under natural light to generate unstable peroxides, which in turn generate chromophore quinone-imide structures, causing the coating to turn yellow. Further oxidation will generate diquinone-imide structures, which eventually turn into amber. Aromatic polyurethane waterproof coatings directly affect the outdoor application areas of polyurethane waterproof coatings.

[0004] With the domestic policy on the emission limit of volatile organic compounds (VOC) in waterproof coatings, as well as the enhancement of people's environmental awareness and the advancement of technology, the application scenarios of tar-based and solvent-based polyurethane waterproof coatings are restricted. In the single-component and two-component polyurethane waterproof coatings on the market, 4,4'-diamino-3,3'-dichlorodiphenylmethane (MOCA) is generally used as a curing agent, but in 2017, MOCA was announced by the World Health Organization as a Class I carcinogen, which seriously endangers the natural environment and human health, further limiting the use of conventional polyurethane waterproof coatings.

[0005] Green curing polyurethane waterproof coatings are mainly polyether-based, solvent-free and environmentally friendly high-grade synthetic polymer waterproof coatings. Compared with traditional tar-based and petroleum asphalt polyurethane waterproof coatings, green curing polyurethane waterproof coatings have the advantages of no solvent volatilization, non-toxic, odorless, pollution-free construction, and rapid curing, which meet the requirements of ecological development and environmental protection. This green curing method reflects the new ideas and new processes for the research and development of polyurethane waterproof coatings, has broad market prospects, and is the research hotspot and difficulty of waterproof products of various enterprises.

[0006] As the exposed polyurethane waterproof coating is used for a longer time, micro cracks that are difficult to observe appear on the surface and inside the material. As the micro cracks spread, macro cracks appear, which directly affect the stability and service life of the polyurethane waterproof layer. By introducing small molecule self-healing groups into the main chain of the polyurethane molecular chain, the micro cracks inside the coating can be repaired, thus improving the service life of the polyurethane waterproof layer.

[0007] Self-healing materials can be divided into intrinsic self-healing materials and external self-healing materials. In external self-healing materials, the repair agent is encapsulated into the material matrix and released to repair the damage when damage occurs. Since external self-healing materials only allow one-time repair at a specific location, their scope of application is limited. However, intrinsic self-healing materials can self-repair an unlimited number of times. But this self-healing process usually requires some external conditions to trigger, such as light, electricity, magnetic field or thermal stimulation. In some cases, these external triggering conditions are easier to obtain and control, but in other cases, such as waterproof materials are generally used in more hidden parts, it is not easy to obtain external triggering conditions.

[0008] CN111234175A discloses a method for preparing a self-repairing waterproof material, which comprises firstly generating a polyurethane / polyurea prepolymer by reacting a polyether or polyester with a monomer containing a diisocyanate group, then using a monomer containing an aromatic disulfide bond as a chain extender to extend the chain to obtain a polyurethane prepolymer having a hydroxyl or amino group at the end group, and then reacting the prepolymer with an isocyanate or NCO-terminated prepolymer to obtain a polyurethane or polyurea elastomer containing an aromatic disulfide bond.

[0009] CN113088178A discloses a high-solid weather-resistant flame-retardant one-component polyurethane waterproof coating and its preparation. The invention replaces aromatic isocyanate with aliphatic isocyanate and adds simple antioxidant and anti-yellowing additives to prepare a weather-resistant polyurethane waterproof coating. The invention adds too little weather-resistant additives and does not improve the weather resistance through physical and chemical synergistic methods. The actual exposure life of the material is short and cannot be applied to large-area exposure projects. Summary of the invention

[0010] In view of the above-mentioned shortcomings of polyurethane waterproof coatings in the prior art, such as great chemical hazard, no weather resistance, no oxygen resistance, great environmental damage and inability to self-heal, the present invention provides a method for preparing a green-curing, highly weather-resistant and self-repairing polyurethane waterproof coating. By adopting aliphatic isocyanate as a raw material, adjusting the isocyanate content and adding a small molecule self-repairing chain extender, the tensile strength of the coating is improved, and the self-repairing ability of cracks inside and on the surface of the coating is given; by adding a hydrophilic chain extender, the oily polyurethane waterproof coating can be stirred with water to become a uniform viscous state, the curing speed of the coating is improved, and the polyurethane chain extension is achieved through a green curing method, so that the waterproof coating is green and environmentally friendly and the mechanical properties of the coating are improved.

[0011] A green curing, highly weather-resistant and self-repairing polyurethane waterproof coating, comprising the following raw materials in parts by weight:

[0012]

[0013] The above-mentioned green curing, highly weather-resistant self-repairing polyurethane waterproof coating also includes the following raw materials in parts by weight:

[0014]

[0015] The weather-resistant and oxygen-resistant additive is any one of a benzotriazole ultraviolet absorber and a hindered amine light stabilizer, or a mixture of the two in any proportion. Preferably, the weather-resistant and oxygen-resistant additive is any one of 2-(2'-hydroxy-5'-methylphenyl)benzotriazole and N,N'-bis(2,2,6,6-tetramethyl-4-piperidinyl)-1,3-benzenedicarbamide, or a mixture of the two in any proportion. The benzotriazole ultraviolet absorber and the hindered amine light stabilizer work synergistically to stabilize the hydrogen bond structure of the polyurethane molecule and capture the free radicals generated during the aging process.

[0016] The above-mentioned polyol oligomer is any one of polyester diol, polyethylene glycol diol, polypropylene glycol diol, polytetramethylene glycol diol, polycarbonate diol, or a mixture of two or more in any proportion; the above-mentioned diisocyanate is any one of isophorone diisocyanate (IPDI), dicyclohexylmethane diisocyanate (HMDI), hexamethylene diisocyanate (HDI), lysine diisocyanate (LDI), or a mixture of two or more in any proportion; the above-mentioned isocyanate content is 3.5-6.5%.

[0017] The hydrophilic chain extender is any one of 2,2-dihydroxymethylpropionic acid (DMPA) and 2,2-dihydroxymethylbutyric acid (DMBA) or a mixture of the two in any proportion; the self-repairing small molecule chain extender is any one of 2-hydroxyethyl disulfide (HEDS) and 5-(2-hydroxyethyl)-6-methyl-aminouracil (HMA).

[0018] The catalyst is any one of an organotin catalyst, a tertiary amine catalyst and an organometallic compound, or a mixture of two or more of them in any proportion. Preferably, the catalyst is dibutyltin dilaurate.

[0019] The above-mentioned inorganic powder filler is any one of heavy calcium carbonate, light calcium carbonate, kaolin, talc, or a mixture of two or more in any proportion; the above-mentioned gas absorbent is any one of calcium hydroxide, sodium hydroxide and cement, or a mixture of two or more in any proportion; the above-mentioned liquid filler is any one of chlorinated paraffin, phthalate or dinonyl phthalate, or a mixture of two or more in any proportion.

[0020] The above-mentioned wetting and dispersing agent is any one of a cationic wetting and dispersing agent and an anionic wetting and dispersing agent, or a mixture of two or more in any proportion. Preferably, the wetting and dispersing agent is a quaternary ammonium salt cationic wetting and dispersing agent; the above-mentioned defoaming agent is any one of a straight-chain aliphatic alcohol series, a silicone series and a fluorine-modified polymer series, or a mixture of two or more in any proportion. Preferably, the defoaming agent is a polysiloxane defoaming agent; the above-mentioned anti-settling agent is any one of fumed silica, organic bentonite and polyamide wax, or a mixture of two or more in any proportion.

[0021] A method for preparing a green curing, highly weather-resistant and self-repairing polyurethane waterproof coating comprises the following steps:

[0022] (1) Add polyol oligomers, gas absorbents, and weather and oxygen resistance additives into the reactor, raise the temperature to 105-120° C., and perform vacuum dehydration for 1-2 hours;

[0023] (2) After the water content is measured to be less than 0.05%, the mixture is cooled to 60° C., and diisocyanate, a hydrophilic chain extender, and a self-repairing small molecule chain extender are added, and the mixture is reacted at 80 to 85° C. for 2 to 3 hours;

[0024] (3) Cool down to 60°C, add catalyst and stir for 30 minutes, seal and discharge to obtain waterproof coating.

[0025] The inorganic powder filler, gas absorbent, liquid filler and wetting dispersant are added in step (1); and the defoamer and anti-settling agent are added in step (3).

[0026] When applying the green-curing, highly weather-resistant and self-repairing polyurethane waterproof coating, add deionized water and stir for 5 to 10 minutes to make the coating become viscous and uniform, and then proceed with the coating construction.

[0027] The mass ratio of deionized water to waterproof coating is (1-3): 10. Insufficient water usage will greatly prolong the curing time of the coating and reduce the mechanical strength; excessive water usage will cause the coating to be loose inside and affect the mechanical strength.

[0028] Compared with the prior art, this application has the following advantages:

[0029] (1) The present invention uses aliphatic isocyanate or alicyclic isocyanate as the hard segment of the polyurethane waterproof coating to improve the weather resistance, yellowing resistance and aging resistance of the polyurethane waterproof coating itself under natural conditions; self-repairing groups are introduced into the polyurethane main chain: 2-hydroxyethyl disulfide (HEDS) and 5-(2-hydroxyethyl)-6-methyl-aminouracil (HMA), and the self-repair of microcracks inside the exposed coating is achieved through the fracture and recombination of reversible groups. The above-mentioned self-repairing small molecule chain extender can realize the rapid self-repair of scratches in the coating under natural conditions.

[0030] (2) Titanium dioxide (TiO2) and weather-resistant and oxygen-resistant additives are added to absorb or shield ultraviolet rays in nature by physical means; alkyl free radicals and amino free radicals generated during the aging process of polyurethane are captured by chemical means to inhibit the aging damage of exposed polyurethane waterproof coatings under natural conditions. Through the synergistic effect of titanium dioxide (TiO2) and weather-resistant and oxygen-resistant additives, the coating surface will not be powdered or cracked after 1000 hours of xenon lamp irradiation.

[0031] (3) The present invention uses water as a curing agent, which not only improves the internal cross-linking degree of the coating and increases the mechanical properties of the coating; but also shortens the surface drying time of the coating and improves the efficiency of engineering construction.

[0032] The present invention adopts aliphatic isocyanate or alicyclic isocyanate with excellent weather resistance and yellowing resistance as the matrix material, and improves the anti-aging ability of the polyurethane waterproof coating by adding nano titanium dioxide and weather and oxygen resistance additives; and introduces reversible reorganization self-repairing groups in the polyurethane prepolymer synthesis process; in the process of using the coating, water is added as a curing agent to react with the residual -NCO group in the coating to achieve rapid curing of the coating and improve the mechanical properties. This green and environmentally friendly curing method completes the internal cross-linking of the polyurethane and improves the mechanical strength of the coating; it speeds up the actual drying time of the coating surface, shortens the construction time, and does not have any health risks. The preparation and production process of the green curing, high weather resistance self-repairing polyurethane waterproof coating of the present invention is simple, low cost, low VOC, low environmental pollution and excellent mechanical properties of the coating, which is conducive to large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 The self-repairing effect diagram of surface scratches after the waterproof coatings of Comparative Example 3 and Examples 1-5 are formed;

[0034] Figure 2 The surface states of the waterproof coatings of Comparative Example 4 and Example 4 after being irradiated by a xenon lamp for 500 hours and 1000 hours;

[0035] Figure 3 It is a comparison chart of the tensile strength of the waterproof coating of Examples 1-5 and Comparative Examples 5-8;

[0036] Figure 4 It is a comparison chart of the water absorption rate of the waterproof coating of comparative example 7 and embodiments 1-5. DETAILED DESCRIPTION

[0037] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solution of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0038] Example 1

[0039] In a reactor equipped with a stirrer, a nitrogen protection device and a reflux condenser, according to the isocyanate content of 3.5, 90 parts of polyethylene glycol diol, 150 parts of light calcium carbonate, 20 parts of calcium hydroxide, 70 parts of liquid chlorinated paraffin, 2 parts of quaternary ammonium salt wetting and dispersing agent, 2 parts of 2-(2'-hydroxy-5'-methylphenyl)benzotriazole and 2 parts of nano titanium dioxide are added, and the temperature is raised to 110°C for vacuum dehydration for 2 hours; after the water content is measured to be lower than 0.05%, the temperature is cooled to 60°C, 15 parts of isophorone diisocyanate, 3 parts of 2,2-dihydroxymethylpropionic acid and 5 parts of 2-hydroxyethyl disulfide are added, and the reaction is carried out at 80°C for 2 hours; the temperature is cooled to 60°C, 1 part of dibutyltin dilaurate, 1 part of polysiloxane defoaming agent and 1 part of fumed silica anti-settling agent are added, and the mixture is stirred for 30 minutes, and the material is sealed and discharged to obtain a waterproof coating.

[0040] Deionized water is added to the prepared waterproof coating, with the mass ratio of the waterproof coating to deionized water being 10:1. Stir for 10 minutes to make the coating become viscous and uniform, and then the coating construction can be carried out.

[0041] Example 2

[0042] In a reactor equipped with a stirrer, a nitrogen protection device and a reflux condenser, according to the isocyanate content of 4.0, 100 parts of polypropylene glycol diol, 140 parts of kaolin, 25 parts of calcium hydroxide, 80 parts of chlorinated paraffin, 2 parts of quaternary ammonium salt wetting and dispersing agent, 2 parts of N,N'-bis(2,2,6,6-tetramethyl-4-piperidinyl)-1,3-benzenedicarbamide and 2 parts of nano titanium dioxide are added, and the temperature is raised to 110°C for vacuum dehydration for 2 hours; after the water content is measured to be lower than 0.05%, the temperature is cooled to 60°C, 18 parts of isophorone diisocyanate, 4 parts of 2,2-dihydroxymethylpropionic acid and 5 parts of 2-hydroxyethyl disulfide are added, and the reaction is carried out at 80°C for 2 hours; the temperature is cooled to 60°C, 1 part of dibutyltin dilaurate, 1 part of polysiloxane defoaming agent and 1 part of fumed silica anti-settling agent are added, and the mixture is stirred for 30 minutes, and the material is sealed and discharged to obtain a waterproof coating.

[0043] Deionized water is added to the prepared waterproof coating, with the mass ratio of the waterproof coating to deionized water being 10:2. Stir for 10 minutes to make the coating become viscous and uniform, and then the coating construction can be carried out.

[0044] Example 3

[0045] In a reactor equipped with a stirrer, a nitrogen protection device, and a reflux condenser, according to the isocyanate content of 4.5, 110 parts of polypropylene glycol diol, 130 parts of heavy calcium carbonate, 25 parts of sodium hydroxide, 90 parts of chlorinated paraffin, 2 parts of quaternary ammonium salt wetting and dispersing agent, 2 parts of (2-(2'-hydroxy-5'-methylphenyl)benzotriazole: N,N'-bis(2,2,6,6-tetramethyl-4-piperidinyl)-1,3-benzenedicarboxylate=1:1) and 2 parts of Nano titanium dioxide is heated to 110°C and vacuum dehydrated for 2 hours; after the water content is measured to be lower than 0.05%, it is cooled to 60°C, 20 parts of dicyclohexylmethane diisocyanate, 5 parts of 2,2-dihydroxymethylpropionic acid and 6 parts of 2-hydroxyethyl disulfide are added, and the reaction is carried out at 80°C for 2 hours; the temperature is cooled to 60°C, 2 parts of dibutyltin dilaurate, 2 parts of polysiloxane defoaming agent and 2 parts of organic bentonite anti-settling agent are added, and stirred for 30 minutes, and the waterproof coating is obtained by sealing the discharge.

[0046] Deionized water is added to the prepared waterproof coating, with the mass ratio of the waterproof coating to deionized water being 10:2. Stir for 10 minutes to make the coating become viscous and uniform, and then the coating construction can be carried out.

[0047] Example 4

[0048] In a reactor equipped with a stirrer, a nitrogen protection device and a reflux condenser, according to the isocyanate content of 4.7, 120 parts of polytetrahydrofuran diol, 120 parts of talc, 30 parts of sodium hydroxide, 100 parts of chlorinated paraffin, 3 parts of quaternary ammonium salt wetting and dispersing agent, 3 parts of (2-(2'-hydroxy-5'-methylphenyl)benzotriazole: N,N'-bis(2,2,6,6-tetramethyl-4-piperidinyl)-1,3-benzenedicarbamide = 2:1) and 3 parts of nano dioxide were added. Titanium is heated to 110°C and vacuum dehydrated for 2 hours; after the water content is measured to be less than 0.05%, it is cooled to 60°C, 25 parts of dicyclohexylmethane diisocyanate, 6 parts of 2,2-dihydroxymethylbutyric acid and 7 parts of 5-(2-hydroxyethyl)-6-methyl-aminouracil are added, and the reaction is carried out at 85°C for 2 hours; the temperature is cooled to 60°C, 2 parts of dibutyltin dilaurate, 2 parts of polysiloxane defoaming agent and 2 parts of organic bentonite anti-settling agent are added, and stirred for 30 minutes, and the waterproof coating is obtained by sealing the discharge.

[0049] Deionized water is added to the prepared waterproof coating, with the mass ratio of the waterproof coating to deionized water being 10:3. Stir for 10 minutes to make the coating become viscous and uniform, and then the coating construction can be carried out.

[0050] Example 5

[0051] In a reactor equipped with a stirrer, a nitrogen protection device and a reflux condenser, according to the isocyanate content of 5.7, 130 parts of polytetrahydrofuran diol, 100 parts of talc, 30 parts of cement, 110 parts of dinonyl phthalate, 4 parts of quaternary ammonium salt wetting and dispersing agent, 4 parts of 2-(2'-hydroxy-5'-methylphenyl)benzotriazole and 4 parts of nano titanium dioxide are added, and the temperature is raised to 110°C for vacuum dehydration for 2 hours; after the water content is measured to be lower than 0.05%, the temperature is cooled to 60°C, 30 parts of hexamethylene diisocyanate, 7 parts of 2,2-dihydroxymethylbutyric acid and 7 parts of 5-(2-hydroxyethyl)-6-methyl-aminouracil are added, and the reaction is carried out at 85°C for 2 hours; the temperature is cooled to 60°C, 2 parts of dibutyltin dilaurate, 2 parts of polysiloxane defoaming agent and 2 parts of polyamide wax anti-settling agent are added, and the mixture is stirred for 30 minutes, and the material is sealed and discharged to obtain a waterproof coating.

[0052] Deionized water is added to the prepared waterproof coating, with the mass ratio of the waterproof coating to deionized water being 10:3. Stir for 10 minutes to make the coating become viscous and uniform, and then the coating construction can be carried out.

[0053] Example 6

[0054] In a reactor equipped with a stirrer, a nitrogen protection device and a reflux condenser, according to the isocyanate content of 4.7, 120 parts of polytetrahydrofuran diol, 3 parts of N,N'-bis(2,2,6,6-tetramethyl-4-piperidinyl)-1,3-benzenedicarbamide and 3 parts of nano-titanium dioxide are added, and the temperature is raised to 110°C for vacuum dehydration for 2 hours; after the water content is measured to be lower than 0.05%, the temperature is cooled to 60°C, 25 parts of dicyclohexylmethane diisocyanate, 6 parts of 2,2-dihydroxymethylbutyric acid and 7 parts of 5-(2-hydroxyethyl)-6-methyl-aminouracil are added, and the reaction is carried out at 80°C for 2 hours; the temperature is cooled to 60°C, 2 parts of dibutyltin dilaurate are added, and the mixture is stirred for 30 minutes, and the material is sealed and discharged to obtain a waterproof coating.

[0055] Deionized water is added to the prepared waterproof coating, with the mass ratio of the waterproof coating to deionized water being 10:3. Stir for 10 minutes to make the coating become viscous and uniform, and then the coating construction can be carried out.

[0056] Comparative Example 1

[0057] The difference between Comparative Example 1 and Example 4 is that toluene diisocyanate is used. Result: The coating surface is yellowed.

[0058] Comparative Example 2

[0059] The difference between Comparative Example 2 and Example 4 is that no nano titanium dioxide and no oxygen-resistant and weather-resistant additive are added. Result: The anti-aging time of the coating is greatly shortened, and powdering and cracking occur in a short time.

[0060] Comparative Example 3

[0061] The difference between Comparative Example 3 and Example 4 is that no self-repairing small molecule chain extender is used. Result: The coating does not have a repairing function.

[0062] Comparative Example 4

[0063] The difference between Comparative Example 4 and Example 4 is that toluene diisocyanate is used, nano titanium dioxide is not added, and oxygen-resistant and weather-resistant additives are not added. Result: The coating surface turns yellow and the anti-aging time is greatly shortened.

[0064] Comparative Example 5

[0065] The difference between Comparative Example 5 and Example 4 is that when the isocyanate content is 2.5%, the tensile strength of the coating decreases and the curing time is prolonged.

[0066] Comparative Example 6

[0067] The difference between Comparative Example 6 and Example 4 is that when the isocyanate content is 7.0%, a large number of bubbles and pores appear on the surface and inside of the coating, resulting in a decrease in the mechanical properties and waterproof properties of the coating.

[0068] Comparative Example 7

[0069] The difference between Comparative Example 7 and Example 4 is that no hydrophilic chain extender is added. Result: It cannot be stirred evenly with water, resulting in the inability to shorten the curing time and improve the mechanical properties through the green curing method (water curing).

[0070] Comparative Example 8

[0071] The difference between Comparative Example 8 and Example 4 is that no deionized water is added as a curing agent during application. Result: The curing time of the coating is greatly prolonged and the mechanical strength is reduced.

[0072] Test Example 1:

[0073] Examples 1-6 of the present invention and comparative examples 1-8 were tested for weather resistance, water resistance, oxygen resistance, water absorption, acid and alkali resistance, coating surface scratch self-repair performance, tensile strength self-repair and self-repair strength repair rate. The specific detection methods are as follows:

[0074] Weather resistance: Use the water resistance test method in GBT19250-2003 national standard: After the product coating is dried, place it in a xenon lamp aging box, control the temperature at 25°C, and the relative humidity at 50%. After 500h and 1000h, observe whether there are defects such as discoloration, blistering, and shedding.

[0075] Tensile strength: The tensile strength test method in the national standard GBT19250-2003 is adopted: the product film is cut into standard dumbbell-shaped tensile specimens, and the test speed is 500±5mm / min.

[0076] Surface drying time: The surface drying time test method in the national standard GBT19250-2003 is adopted: the wet film thickness is 0.5mm±0.1mm, and the surface drying time of the paint is judged by lightly touching the surface of the coating with a finger.

[0077] Drying time: The surface drying time test method in GBT19250-2003 national standard is adopted: the wet film thickness is 0.5mm±0.1mm, and the coating drying time is judged by lightly touching the bottom layer and inner film of the coating with your fingers.

[0078] Water resistance: The water resistance test method in the national standard GBT19250-2003 is used: the product coating is dried and completely immersed in deionized water for 240 hours, and then the tensile strength retention rate of the coating is tested.

[0079] Oxygen resistance: The water resistance test method in the national standard GBT19250-2003 is used: after the product coating is dried, place it in an electric blast oven at 80°C for 168 hours, and then test the tensile strength retention rate of the coating.

[0080] Water absorption rate: Use the water resistance test method in the national standard GBT19250-2003: After the product coating is dried, completely soak it in deionized water for 240 hours, and calculate the water absorption rate of the coating.

[0081] Acid and alkali resistance: The water resistance test method in the national standard GBT19250-2003 is used: After the product coating is dried, it is completely immersed in a 10% concentration of NaOH and H2SO4 solution for 240 hours, and then the tensile strength retention rate of the coating is tested.

[0082] Scratch self-repair performance and repeated self-repair test: After the composite coating product film is dry, use a scalpel to make a small scratch on the coating surface, and self-repair under natural conditions until the small crack disappears, and record the repair time. After the scratch self-repairs, make another small crack at the same position, repeat the above operation, and observe whether the crack can self-repair.

[0083] Self-repairing tensile strength test: Use a scalpel to cut the dumbbell-shaped tensile specimen in the middle, press the broken surfaces together for 30 seconds, place them under natural conditions to self-repair for 80 minutes, and test the tensile strength with a universal testing machine.

[0084] Self-repair strength recovery rate: The test records that the tensile strength of the dumbbell-shaped composite coating before self-repair is δ0, the tensile strength after self-repair is δ1, and the self-repair strength recovery rate = δ1 / δ0*100%.

[0085] The performance test results are shown in Table 1 below:

[0086] Table 1

[0087]

[0088]

[0089] Table 1 continued:

[0090]

[0091]

[0092] It has been verified that after the waterproof coating of the present invention is cured into a film, the weather resistance, tensile strength, water resistance, and acid and alkali resistance of Examples 1-5 are greatly improved compared to the comparative example. Judging from various properties, the performance of Example 4 is relatively better.

[0093] According to the results in Table 1, the comparison between the results of Example 4 and Comparative Example 3 shows that after adding the self-repairing chain extender, the waterproof coating has multiple microcrack self-repair capabilities under outdoor natural conditions, and the mechanical strength repair rate of the fractured specimen can reach more than 90%; Figure 1 It can be seen that under natural conditions, the surface scratches of the coatings of Examples 1-5 can be self-repaired in a short time, and the experiment proves that the coating has the ability to self-repair repeatedly. In Comparative Example 3, there is no self-repairing chain extender inside, the surface scratches cannot be self-repaired, and the repair efficiency of the broken sample is 0%. The repair efficiency of the broken samples of the embodiments can reach more than 90%, and the coating has excellent repair efficiency and ability.

[0094] Compared with Comparative Example 4, after using aliphatic isocyanate or alicyclic isocyanate and adding nano titanium dioxide and oxygen-resistant weathering additives in Example 4 of the present application, the aging resistance of the coating is greatly improved. After 1000 hours of xenon lamp irradiation, there is no discoloration, blistering and wrinkling on the surface, and it has excellent weather resistance. Figure 2 As shown; in Comparative Example 4, obvious cracks appeared on the coating surface after 500 hours of xenon lamp irradiation, and the cracks on the coating surface deepened and became powdery after 1000 hours of irradiation.

[0095] Figure 3It is a tensile strength comparison chart of the waterproof coating of Examples 1-5 and Comparative Examples 5-8. According to the results of Table 1 and from the figure, it can be seen that the isocyanate content in Comparative Example 5 is relatively low, resulting in a smaller proportion of hard segments in the molecular chain segments and a lower tensile strength. The isocyanate content in Comparative Example 6 is relatively high, and pores appear on the surface and inside of the coating after curing, resulting in a loose coating inside and reducing the tensile strength of the coating. Comparative Example 7 does not add a hydrophilic chain extender, resulting in the coating being unable to be stirred evenly with water, affecting the reaction chain extension, and reducing the tensile strength of the coating. Comparative Example 8 does not extend the chain and cure by adding water, resulting in a reduction in the proportion of hard segments in the molecular weight, extending the coating curing time and reducing the tensile strength of the coating.

[0096] Figure 4 This is a comparison chart of the water absorption of the waterproof coating of Example 7 and Examples 1-5. From the figure, we find that the water absorption of the comparative example is 0.5%, while the water absorption of Examples 1-5 is much higher than that of the comparative example. The oily polyurethane improves its compatibility with water by adding a hydrophilic chain extender, and a uniform and viscous waterproof coating can be formed by physical stirring. The addition of a hydrophilic group leads to an increase in the water absorption of the coating. The water absorption of the coating of Examples 1-5 can meet the national standard GBT19250-2003 through the water absorption test.

[0097] At the same time, the comparison results between Comparative Example 8 and Example 4 show that Example 4 uses green curing to react water as a curing agent with isocyanate, thereby increasing the hard segment ratio in the molecular chain and improving the tensile strength of the coating.

[0098] In summary, the present application avoids the yellowing of polyurethane caused by quinone structure by selecting aliphatic isocyanate as the raw material; by adjusting the isocyanate content and adding small molecule self-healing chain extenders, the tensile strength of the coating is improved, and the coating is endowed with the ability to self-repair cracks inside and on the surface; by adding hydrophilic chain extenders, the oily polyurethane waterproof coating can be stirred with water to become a uniform viscous state, and the polyurethane chain extension is completed by green curing to increase the mechanical strength of the coating, thereby improving the greenness and environmental protection of the waterproof coating.

[0099] The green curing, highly weather-resistant and self-repairing polyurethane waterproof coating produced by the present invention has excellent performance, good system compatibility, low raw material cost, high production efficiency, easy industrialization, and wide application. No toxic solvent is released during the entire process, and the coating is a non-toxic and pollution-free water-based polyurethane coating.

[0100] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A green curing, highly weather-resistant, self-repairing polyurethane waterproof coating, characterized in that: Including the following raw materials by mass:

2. A green curing, highly weather-resistant, self-repairing polyurethane waterproof coating according to claim 1, characterized in that: The following raw materials are also included:

3. A green curing, highly weather-resistant, self-repairing polyurethane waterproof coating according to claim 1, characterized in that: The polyol oligomer is any one of polyester diol, polyethylene glycol diol, polypropylene glycol diol, polytetramethylene glycol diol, polycarbonate diol, or a mixture of two or more of them in any proportion; the diisocyanate is any one of isophorone diisocyanate, dicyclohexylmethane diisocyanate, hexamethylene diisocyanate, lysine diisocyanate, or a mixture of two or more of them in any proportion; the isocyanate content is 3.5-6.5%.

4. A green curing, highly weather-resistant, self-repairing polyurethane waterproof coating according to claim 1, characterized in that: The hydrophilic chain extension is any one of 2,2-dihydroxymethylpropionic acid and 2,2-dihydroxymethylbutyric acid or a mixture of the two in any proportion; the self-repairing small molecule chain extension is any one of 2-hydroxyethyl disulfide and 5-(2-hydroxyethyl)-6-methyl-aminouracil.

5. The green curing, highly weather-resistant, self-repairing polyurethane waterproof coating according to claim 1, characterized in that: The weather-resistant and oxygen-resistant additive is any one of a benzotriazole ultraviolet absorber and a hindered amine light stabilizer, or a mixture of the two in any proportion; the catalyst is any one of an organic tin catalyst, a tertiary amine catalyst, and an organic metal compound, or a mixture of two or more in any proportion.

6. A green curing, highly weather-resistant, self-repairing polyurethane waterproof coating according to claim 2, characterized in that: The inorganic powder filler is any one of heavy calcium carbonate, light calcium carbonate, kaolin, talc, or a mixture of two or more in any proportion; the gas absorbent is any one of calcium hydroxide, sodium hydroxide, and cement, or a mixture of two or more in any proportion; the liquid filler is any one of chlorinated paraffin, phthalate, or dinonyl phthalate, or a mixture of two or more in any proportion.

7. A green curing, highly weather-resistant, self-repairing polyurethane waterproof coating according to claim 2, characterized in that: The wetting and dispersing agent is any one of a cationic wetting and dispersing agent and an anionic wetting and dispersing agent, or a mixture of two or more in any proportion; the defoaming agent is any one of a linear aliphatic alcohol series, a silicone series, and a fluorine-modified polymer series, or a mixture of two or more in any proportion; the anti-settling agent is any one of fumed silica, organic bentonite, and polyamide wax, or a mixture of two or more in any proportion.

8. A method for preparing a green curing, highly weather-resistant and self-repairing polyurethane waterproof coating according to any one of claims 1 to 7, characterized in that: The following steps are involved: (1) Add polyol oligomers, nano titanium dioxide, and weather-resistant and oxygen-resistant additives into a reactor, raise the temperature to 105-120° C., and perform vacuum dehydration for 1-2 hours; (2) After the water content is measured to be less than 0.05%, the mixture is cooled to 60° C., and diisocyanate, a hydrophilic chain extender, and a self-repairing small molecule chain extender are added, and the mixture is reacted at 80 to 85° C. for 2 to 3 hours; (3) Cool down to 60°C, add catalyst and stir for 30 minutes, seal and discharge to obtain waterproof coating.

9. The method for preparing a green curing, highly weather-resistant and self-repairing polyurethane waterproof coating according to claim 8, characterized in that: The inorganic powder filler, gas absorbent, liquid filler and wetting dispersant are added in step (1); and the defoaming agent and anti-settling agent are added in step (3).

10. The method for applying a green curing, highly weather-resistant and self-repairing polyurethane waterproof coating according to any one of claims 1 to 7, characterized in that: When the waterproof coating is applied, deionized water is added and stirred for 5 to 10 minutes to make the coating become viscous and uniform, and then the coating construction can be carried out; the mass ratio of the deionized water to the waterproof coating is (1-3):10.

Citation Information

Patent Citations

  • Self-emulsifying type water curing environment-friendly polyurethane waterproof paint

    CN105001776A

  • Preparation method of waterborne polyurethane capable of selfreparing

    CN105885002A

  • Single-component exposed polyurethane waterproof paint and preparation method thereof

    CN106381047A

Cited By

  • Preparation process of exposed rubber asphalt waterproof coating

    CN120272113A

  • Transparent high-strength silane modified polyether waterproof coating and preparation method thereof

    CN121203520A

  • Weather-resistant anti-aging coating for coastal port crane and preparation method of weather-resistant anti-aging coating

    CN122326100A