Glue material for coating oriented silicon steel, rubber roller and preparation method
By designing high-performance oriented silicon steel coating materials and improved rubber roller preparation technology, the problem of short application cycle of coating rollers in the prior art is solved, and a longer service life and a more uniform coating effect are achieved. Promote the development of the domestic silicon steel industry.
Patent Information
- Application Number
- CN202410952193.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-16
- Publication Date
- 2024-11-08
AI Technical Summary
The coating rollers of the existing oriented silicon steel production lines have a short service life, which is difficult to meet the needs of high-quality coatings, and are relatively high in cost, which affects the development of the domestic industry.
Designed a oriented silicon steel coating material including nitrile rubber, carbon black, zinc oxide, plasticizer, inorganic filler, wear-resistant resin, vulcanizing agent, accelerator and anti-coke agent, through reasonable proportion and sulfurization. The process improves the hardness, wetting and corrosion resistance of the rubber material, and uses UTH filtration and wide sheet rubber strip forming method to coat the rubber roller core to enhance the wear resistance and service life of the rubber roller.
It significantly improves the reuse times and usage cycle of rubber rollers, meets the requirements of continuous use for more than 6 days and more than 10 cycles of grooves, reduces production costs, improves coating uniformity and corrosion resistance, and is suitable for Domestic oriented silicon steel production line.
Smart Images

Figure BDA0004947528870000071 
Figure BDA0004947528870000081
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of rubber rollers, and more specifically, relates to a rubber material for coating oriented silicon steel, a rubber roller and a preparation method thereof. Background Art
[0002] With the requirements of global carbon emission policies, China's carbon emission planning, the rapid development of the domestic new energy vehicle industry and the high-end development of the photovoltaic industry, the demand for oriented silicon steel at home and abroad is increasing due to its superior performance of low energy consumption, especially high-quality oriented silicon steel is currently in short supply. In the early years, my country introduced silicon steel production lines from Europe, the United States, Japan and South Korea, which were absorbed and improved by domestic technicians. Now my country is able to independently design and manufacture silicon steel production lines, and there are hundreds of production lines in operation and construction.
[0003] In the production process of oriented silicon steel, a uniform isolation layer needs to be coated on the surface of the oriented silicon steel plate. In the prior art, rubber rollers with different groove types, groove depths and groove widths are used to coat the surface of the oriented silicon steel plate. The rubber rollers originally imported from Europe, the United States, Japan and South Korea are not conducive to the development of the domestic oriented silicon steel industry due to their long production cycle and high prices. Therefore, many domestic manufacturers are currently developing them. However, the products developed by domestic manufacturers cannot meet the needs of domestic companies. There are problems such as difficulty in groove forming, short one-time use cycle (within 3 days), difficulty in repeated use (less than 10 times) and uneven coating film thickness. Improving the rubber roller can reduce the difficulty of groove forming, improve its one-time use cycle, number of repeated uses and coating uniformity, and reduce production costs. The significance of promoting the development of the domestic oriented silicon steel industry is self-evident.
[0004] Chinese patent document 201420736762.3 discloses a magnesium oxide coating device for an oriented silicon steel production line, which enables the lower coating roller to bring sufficient suspension to both ends of the roller, thereby increasing the thickness of the lower magnesium oxide coating and ensuring the uniformity of the coating. However, it does not provide a solution or any technical inspiration for the problem of short service life of the rubber roller. Summary of the invention
[0005] 1. Problem to be solved
[0006] In view of the problem of short service life of coating rollers in existing oriented silicon steel production lines, the present invention provides a rubber material for coating oriented silicon steel, a rubber roller and a preparation method thereof, which can improve the uniformity of roller surface hardness, the wettability of silicon steel coating liquid and the corrosion resistance.
[0007] 2. Technical solution
[0008] In order to solve the above problems, the technical solution adopted by the present invention is as follows:
[0009] In a first aspect, the present invention provides a rubber compound for coating oriented silicon steel, wherein the rubber compound is used for coating the surface of oriented silicon steel to form a coating. The rubber compound comprises the following raw material components calculated by weight:
[0010] Nitrile rubber: 50-55 parts;
[0011] Carbon black: 20-25 parts;
[0012] Zinc oxide: 1-10 parts;
[0013] Stearic acid: 0.5-1 part;
[0014] Plasticizer: 1.5-5.5 parts;
[0015] Polyethylene glycol: 1.5-2.5 parts;
[0016] Tackifier: 1.5-2.3 parts;
[0017] Inorganic filler: 5.4-10.6 parts;
[0018] Wear-resistant resin: 4-10.6 parts;
[0019] Vulcanizing agent: 0.5-2.1 parts;
[0020] Accelerator: 0.25-1.8 parts;
[0021] Anti-scorching agent: 0.5-1 part.
[0022] By adopting the above technical scheme, the wear resistance and hardness of nitrile rubber are good, which can improve the performance of the rubber compound. At the same time, the present invention makes reasonable adjustments in the selection and ratio of raw materials, so that its various performances, such as wettability, corrosion resistance, and friction resistance are all good, meeting the requirements of the oriented silicon steel coating production line. After long-term friction with the steel plate, the rubber compound can still ensure the groove shape and groove depth, and can meet certain production requirements of online use time and steel passing amount. Specifically, it meets the requirements of a continuous use cycle of more than 6 days on the line at one time, and more than 10 cycles of grooving and use, which is far longer than the 3-day use cycle in the prior art.
[0023] The above-mentioned nitrile rubber may be imported from abroad or produced domestically.
[0024] Furthermore, the carbon black is carbon black for rubber.
[0025] It should be noted that carbon black for rubber is divided into channel black, furnace black and thermal cracking black according to the production method.
[0026] Furthermore, the plasticizer includes one or more of petroleum plasticizers, coal tar plasticizers, pine tar plasticizers, fat plasticizers, and synthetic plasticizers.
[0027] Preferably, the plasticizer is an environmentally friendly, non-polluting plasticizer among synthetic plasticizers.
[0028] The reason for adopting the above scheme as the preferred scheme is that the environmentally friendly and non-polluting plasticizer has low toxicity and good biodegradability, which is beneficial to improving the safety of the rubber compound and is environmentally friendly.
[0029] Furthermore, the above-mentioned tackifier includes one or more of terpene resin C5 and terpene resin C9.
[0030] The reason for adopting the above technical solution is that the thermal stability, bonding performance, solubility, chemical stability and plasticity of terpene resin C5 and terpene resin C9 are all good, which is beneficial to improving the processing performance of the rubber compound.
[0031] Furthermore, the inorganic filler includes one or more of zinc oxide, magnesium oxide, white carbon black and titanium dioxide.
[0032] Preferably, the inorganic filler is activated zinc oxide.
[0033] The reason for adopting the above technical solution as the preferred solution is that compared with ordinary zinc oxide, active zinc oxide has better dispersibility, chemical activity and stability, and the binding force between active zinc oxide and rubber is stronger, which helps to improve the mechanical properties of the rubber.
[0034] Furthermore, the wear-resistant resin includes one or more of epoxy resin, phenolic resin and acrylic resin.
[0035] For example, the wear-resistant resin is the GD-17 resin or PR12687 resin produced by Nanjing Golden Company.
[0036] The reason for adopting the above technical solution is that the wear-resistant resin can improve the wear resistance and hardness of the rubber compound, and extend the single-on-line use period and cyclic use performance.
[0037] Furthermore, the above-mentioned vulcanizing agent includes one or more of elemental sulfur vulcanizing agent, sulfur donor vulcanizing agent, peroxide vulcanizing agent, metal oxide vulcanizing agent, quinone derivative resin vulcanizing agent, and amine compound vulcanizing agent.
[0038] Furthermore, the above-mentioned vulcanizing agent includes one or both of an elemental sulfur vulcanizing agent and a sulfur donor vulcanizing agent.
[0039] The reason for adopting the above technical solution is that compared with other vulcanizing agents, elemental sulfur vulcanizing agents have better comprehensive physical and chemical properties, low cost and wide application; while sulfur donor vulcanizing agents have the advantages of safe operation and good heat aging resistance.
[0040] Furthermore, the above-mentioned vulcanizing agent is S-80.
[0041] The reason for adopting the above technical solution is that S-80 is highly efficient, can quickly promote the vulcanization reaction of rubber, shorten the vulcanization time, improve production efficiency, and has good thermal stability, aging resistance, mechanical properties, and processing performance, and has low cost.
[0042] Furthermore, the above-mentioned accelerator includes: accelerator CZ: 0.15-0.9 parts; accelerator DTDM: 0.1-0.9 parts.
[0043] Furthermore, the above-mentioned anti-scorching agent includes one or more of an organic acid anti-scorching agent, a nitroso compound anti-scorching agent and a sulfonamide anti-scorching agent.
[0044] Furthermore, the above-mentioned anti-scorching agent is CTP.
[0045] Furthermore, the hardness Shore A of the rubber compound is 61 to 63 degrees.
[0046] Furthermore, the tear strength of the above-mentioned rubber material is ≥8MPa.
[0047] Furthermore, the rebound of the above rubber material is ≥40%.
[0048] Furthermore, the Akron abrasion of the above rubber compound is ≤0.30 cubic millimeter / 1.61 kilometer.
[0049] Furthermore, the two-plate tearing strength of the rubber material is ≥6Pa, and the rubber failure type is R type.
[0050] Furthermore, the weight change rate of the above-mentioned rubber material after the corrosion resistance test of oriented silicon steel liquid is ≤1%, and the volume change rate is ≤1%.
[0051] Furthermore, the corrosion resistance test conditions of the oriented silicon steel liquid are: temperature: 20°C; immersion time: 168 hours.
[0052] In a second aspect, the present invention provides a rubber roller, comprising a roller core and the aforementioned rubber material, wherein the rubber material covers the roller core.
[0053] Furthermore, the roller core is made of carbon steel or stainless steel.
[0054] In a third aspect, the present invention provides a method for preparing the aforementioned rubber roller, comprising the following steps:
[0055] S1. Banburying: After plasticizing the nitrile rubber, carbon black, inorganic filler, zinc oxide, stearic acid, polyethylene glycol, wear-resistant resin and tackifier are added and mixed, and then the plasticizer is added and mixed, the plug is lifted, the rubber is discharged, and the mixing is stopped to obtain a masterbatch after banburying;
[0056] S2. Filtration: The masterbatch after mixing is filtered using UTH filtration technology to obtain a filtered masterbatch;
[0057] S3. Sulfur refining: The filtered masterbatch is placed on the roller of the mixing mill, and the compounding agents are added: sulfur, accelerator, scorch retarder, and the compounding agents are all eaten into the masterbatch and then the knife is turned over and the rubber is finally obtained by sheeting;
[0058] S4. Wrapping rubber: The rubber material is coated on the roller core to obtain a rubber roller;
[0059] S5. Vulcanization in an autoclave: The rubber roller coated in step S4 is sent to an autoclave for vulcanization;
[0060] S6. Turning and grinding: After the rubber roller vulcanized in step S5 is cooled to room temperature, it is subjected to turning and grinding.
[0061] Furthermore, the above step S1 is specifically as follows:
[0062] Place the nitrile rubber in an internal mixer according to the proportion and plasticize for 80-100 seconds, then add carbon black, inorganic filler and tackifier and mix for 50-60 seconds, then add plasticizer and mix for 120-160 seconds, then lift the plug, and drain the rubber after 150-200 seconds, the discharge temperature is 120-150℃, and leave it for 24hr-48hr to obtain a masterbatch.
[0063] Furthermore, in the above step S1, the mastication time is 90-100s.
[0064] Furthermore, in the above step S1, the plug-lifting time is 150-160s.
[0065] Furthermore, the filtration in the above step S2 uses a filter screen with 80-160 meshes.
[0066] Preferably, the filtration in the above step S2 uses a 160-mesh filter.
[0067] Preferably, the filtration in the above step S2 uses a two-layer filter.
[0068] By adopting the above technical solution, the UTH filtration technology can ensure that there are no impurities in the masterbatch, and in the grooving step of the rubber compound, the uniformity and integrity of the thread can be ensured.
[0069] Furthermore, the above step S3 is specifically as follows:
[0070] After the masterbatch is left to rest, vulcanization is performed: the masterbatch in the above step S2 is placed on the roller of the mixing mill, and after the surface of the masterbatch roller is smooth and flat, compounding agents are added: sulfur, accelerator CZ, accelerator DTDM, and anti-scorch agent CTP. After all the above compounding agents are mixed into the masterbatch, the mixing is started, and the rubber material is rolled into 2-3 triangle bags and 3 rolls before being produced into strips.
[0071] Furthermore, the above step S4 is specifically as follows:
[0072] The rubber material is fed into a screw extruder, the die of the screw extruder is in a sheet shape, and the rubber material is extruded into a film with a thickness of 1-2mm and a width of 60-70mm through the sheet-shaped die, and the film overlapping degree is 0-10m; after the film is uniform, the rotary rubber wrapping machine is started, and the film is wrapped layer by layer on the metal roller core until the thickness of the single side of the rubber wrapping reaches 30-35mm, and isolation paper and nylon water cloth are wrapped on the rubber surface to obtain a rubber roller.
[0073] The present invention adopts a wide thin rubber strip molding method, which is an unconventional winding molding method. Specifically, the molding method of the rubber material is: the screw extruder adopts a thin sheet-shaped die, which reduces the difference in resistance at different positions of the rubber section during the extrusion process, so that the extruded rubber material is evenly distributed, the adhesion between layers is good during the rubber coating process, the material is uniform, the surface quality of the coated steel plate each time and the one-time steel passing amount are basically consistent, and the surface coating thickness of the oriented silicon steel can be met to be 20 to 40 μm.
[0074] Furthermore, after the above step S3 and before step S4, the temperatures of the screw extruder barrel, screw and die head equipment are preheated to 50° C., 60° C. and 50° C. respectively; during the encapsulation process, the temperature of the extruded thin film is controlled to be ≤90° C.
[0075] Furthermore, the above step S5 is specifically as follows:
[0076] The rubber roller obtained in step S4 is sent into a vulcanization tank. After the tank door is closed, steam is introduced into the vulcanization tank and vulcanization is performed by gradually increasing the temperature in a stepwise manner and maintaining the temperature for a long time. While introducing steam, the compressed air valve is opened and compressed air is introduced so that the pressure in the vulcanization tank reaches 0.45-0.50 MPa within 0.5 hr.
[0077] Furthermore, in the above step S5, the stepwise temperature increase and heat preservation for a long time heating vulcanization procedure is: first increase the temperature to 80-90°C, and keep it at 80-90°C for 1hr to 1.5hr; then increase the temperature to 90-100°C, and keep it at 90-100°C for 1hr to 2hr; then increase the temperature to 120-130°C, and keep it at 120-130°C for 1hr; then increase the temperature to 150-155°C, and keep it at 150-155°C for 6hr.
[0078] Furthermore, in the above step S5, the pressure in the vulcanization tank is maintained at 0.45-0.50 MPa during the entire heating and vulcanization process.
[0079] The method of gradually increasing the temperature and keeping the temperature for a long time during vulcanization is adopted, so that the vulcanization degree inside and on the surface of the rubber roller is uniform and the material properties are consistent; at the same time, the compressed air is added during the vulcanization process to ensure that there is enough pressure in the vulcanization tank, which increases the bonding strength between the rubber layers and between the rubber layers and the roller core; the small molecular gas generated during the rubber vulcanization process is slowly discharged from the rubber material to prevent the formation of pores in the rubber layer.
[0080] Furthermore, the above step S6 is specifically as follows:
[0081] The rubber roller vulcanized in step S5 is naturally cooled to room temperature indoors, processed by a PCD rubber turning tool, and then fine-processed by a special grinder.
[0082] 3. Beneficial effects
[0083] Compared with the prior art, the present invention has the following beneficial effects:
[0084] The present invention provides a rubber material, a rubber roller and a preparation method for improving the uniformity of roller surface hardness, wettability of silicon steel coating liquid and corrosion resistance of coating liquid of an oriented silicon steel coated rubber roller in the prior art, so that the rubber material has better reusability.
[0085] Specifically, the present invention also has the following beneficial effects:
[0086] (1) The rubber roller provided by the present invention has a reasonable raw material ratio, good wettability, corrosion resistance, friction resistance, and uniform film thickness. It can cope with the problems of liquid corrosion and high-speed friction of steel plates in the oriented silicon steel production line. After long-term friction with the steel plate, it can still ensure the groove shape and groove depth, and can meet certain production requirements for online use time and steel passing amount. The rubber roller of the present invention has been put into use on different production lines of different manufacturers in China, meeting the requirements of continuous use cycle of more than 6 days on line at one time, more than 10 cycles of groove engraving and use, far exceeding the 3-day use cycle in the prior art. The uniformity of film thickness, online use cycle and steel passing amount all exceed imported products, and has been widely used in major domestic silicon steel production lines.
[0087] (2) In the preparation method of the rubber roller provided by the present invention, by studying the material formula design, rubber coating process, vulcanization process, turning and grinding process, etc., the raw materials are fully dispersed and fused during rubber mixing, the hardness error inside and outside the rubber roller is plus or minus 1 degree (62±1 Shore A), the material distribution consistency is high, and the roller surface roughness consistency is high, which meets the requirements of various manufacturers for surface processing of various groove shapes, various groove depths (0~3mm) and various groove widths (0.1~1.0mm) of oriented silicon steel coated rollers, thereby ensuring that the groove engraving quality of rubber rollers from different manufacturers is better. DETAILED DESCRIPTION
[0088] It should be noted that, unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by technicians in the technical field to which the present invention belongs; the term "and / or" used herein includes any and all combinations of one or more related listed items.
[0089] If the specific conditions are not specified in the examples, the experiments were carried out under conventional conditions or conditions recommended by the manufacturer. If the manufacturers of the reagents or instruments are not specified, they are all conventional products that can be purchased commercially.
[0090] As used herein, the term "about" is used to provide flexibility and imprecision associated with a given term, measurement or value. The degree of flexibility for a particular variable can be easily determined by one skilled in the art.
[0091] As used herein, "adjacent" refers to the proximity of two structures or elements. Specifically, elements identified as "adjacent" can be adjacent or connected. Such elements can also be close to or in proximity to each other without necessarily touching each other. In some cases, the precise degree of proximity can depend on the specific context.
[0092] As used herein, the term "at least one of" is intended to be synonymous with "one or more of." For example, "at least one of A, B, and C" expressly includes only A, only B, only C, and combinations of each thereof.
[0093] Concentration, amount and other numerical data can be presented in range format herein.It should be understood that such range format is only used for convenience and simplicity, and should be flexibly interpreted as not only including the numerical value clearly described as range limit, but also including all single numerical values or sub-ranges contained in the range, just as each numerical value and sub-range are clearly described.For example, the numerical range of about 1 to about 4.5 should be interpreted as not only including the limit value of 1 to about 4.5 clearly described, but also including single numerals (such as 2,3,4) and sub-ranges (such as 1 to 3,2 to 4, etc.).The same principle is applicable to the scope of only narrating a numerical value, such as "less than about 4.5", which should be interpreted as including all the above-mentioned values and ranges.In addition, no matter how the breadth of the described range or feature is, this explanation should be applicable.
[0094] Any steps described in any method or process claim (for example, steps S1, S2, S3... or steps (1), (2), (3)... or steps 1), 2), 3)...) may be performed in any order and are not limited to the order presented in the claims.
[0095] The method+function or step+function limitation shall be adopted only when all of the following conditions are present in a particular claim limitation: S1 explicitly recites "a method for..." or "a step for..."; S2 explicitly recites the corresponding function. The structure, material, or action supporting the method+function is explicitly recited in the description herein. Therefore, the scope of the present invention shall be determined solely by the appended claims and their legal equivalents, rather than by the description and examples given herein.
[0096] The present invention is further described below in conjunction with specific embodiments.
[0097] In the following examples, if no specific conditions are specified, the experiments were carried out under conventional conditions or conditions recommended by the manufacturer. The reagents or instruments used, if no manufacturer is specified, are all conventional products that can be purchased commercially.
[0098] Examples 1 to 3
[0099] Examples 1 to 3 respectively provide a rubber compound for coating oriented silicon steel, which is used to apply a coating to the surface of oriented silicon steel to form a coating. The raw material components of the rubber compound in each example are shown in Table 1, calculated by weight.
[0100] Table 1 Raw material components of the rubber compound in Examples 1 to 3
[0101] Raw materials / Example Example 1 Example 2 Example 3 Nitrile rubber (kg) 25.00 26.00 27.50 Carbon black (kg) 10.00 11.00 12.5 Zinc oxide (kg) 0.50 3.00 5.00 Stearic acid(kg) 0.25 0.40 0.50 Plasticizer(kg) 0.75 1.50 2.75 Polyethylene glycol (kg) 0.75 1.0 1.25 Thickener(kg) 0.75 1.00 1.15 Inorganic filler (kg) 2.70 3.50 5.30 Wear-resistant resin (kg) 2.00 4.00 5.30 Vulcanizing agent S-80 (kg) 0.25 0.50 1.05 Accelerator DTDM (kg) 0.05 0.35 0.45 Accelerator CZ(kg) 0.25 0.35 0.45 Anti-scorch agent CTP (kg) 0.25 0.35 0.50
[0102] In Examples 1 to 3, the nitrile rubber is a general-purpose medium-low acrylonitrile rubber; the carbon black is Cabot high-wear-resistant carbon black; the zinc oxide is active zinc oxide; the stearic acid is industrial-grade stearic acid; the plasticizer is a NEO-T model product of Shanghai Aijing Company; the polyethylene glycol is PEG4000; the tackifier is a C9 tackifying resin; the inorganic filler is titanium dioxide from Shanghai Pinsheng; the wear-resistant resin is a GD-17 model product of Nanjing Gordon Company; the vulcanizer S-80 is an S-80 product of Guangzhou Lida Rubber Raw Materials Trading Co., Ltd.; the accelerator DTDM is a DTDM product of Henan Longji Chemical Co., Ltd.; the accelerator CZ is a CBS model product of Shanghai Disen Chemical; the anti-scorching agent CTP is a CTP-80 model product of Henan Kailun Company.
[0103] The performance parameters of the rubber materials in Examples 1 to 3 (hardness, tensile strength, rebound, Akron abrasion, two-plate tearing strength, rubber failure type, weight change rate, volume change rate) and the usage of the coated roller core to prepare a rubber roller for coating oriented silicon steel (one-time use time, number of repeated uses) are shown in Table 2.
[0104] Table 2 Test results of rubber properties in Examples 1 to 3
[0105]
[0106]
[0107] The test methods for each performance parameter refer to the following standards:
[0108] Hardness: GB / T 531.1-2008;
[0109] Breaking strength: GB / T 528-2009;
[0110] Rebound: GB / T 1681-2009;
[0111] Akron wear: GB / T 1689-2014;
[0112] Two-plate tearing strength: GB / T 11211-2009;
[0113] Rubber failure type: GB / T 11211-2009;
[0114] Oriented silicon steel liquid corrosion resistance test (volume change rate and weight change rate): GB / T 1690-2010;
[0115] The corrosion resistance test conditions of oriented silicon steel liquid are: temperature: 20℃; immersion time: 168 hours.
[0116] Example 4
[0117] This embodiment provides a rubber roller, which comprises a roller core and the rubber material in Embodiment 1, wherein the rubber material covers the roller core. The roller core is made of 45 carbon steel or stainless steel.
[0118] Example 5
[0119] This embodiment provides a method for preparing a rubber roller. The rubber roller as described in Example 1 can be prepared by the method in this embodiment. The method includes the following steps:
[0120] Step 1: Internal mixing: Place the rubber in an internal mixer according to the ratio and plasticize for 90 seconds, then add carbon black, inorganic filler, zinc oxide, stearic acid, polyethylene glycol, wear-resistant resin and tackifier and mix for 60 seconds, then add plasticizer and mix for 150 seconds, then lift the plug, and drain the rubber after 190 seconds, the discharge temperature is 135℃, and the parking time is 24 hours to obtain the masterbatch.
[0121] Step 2: Filtration: Use two layers of 160 mesh filter screens to filter the masterbatch to obtain the filtered masterbatch, and the above filtration adopts UTH filtration technology;
[0122] Step 3: Add sulfur and start refining: Put the masterbatch aside for sulfur addition: Put the filtered masterbatch on the roller of the mixing mill, and add the compounding agents after the masterbatch roller surface is smooth and flat: sulfur, accelerator CZ, accelerator DTDM, anti-scorch agent CTP, and start refining after all the above compounding agents are mixed into the masterbatch. Make 2-3 triangle bags and 3 rolls of the rubber material and then produce strips;
[0123] Step 4: Wrapping and rubber coating: Preheat the barrel, screw and die head of the screw extruder to 50℃, 60℃ and 50℃ respectively; during the rubber coating process, control the temperature of the thin film to be ≤90℃. Feed the rubber into the screw extruder, the die of the screw extruder is a thin sheet, and extrude the rubber into a film with a thickness of 1.5mm and a width of 67mm through the thin sheet die, and the film overlap is 6m; after the film is uniform, start the rotary rubber coating machine, and wrap the film layer by layer on the metal roller core until the thickness of the single side of the rubber coating reaches 34mm. After the rubber coating is completed, wrap the isolation paper and nylon water cloth on the rubber surface to obtain a rubber roller;
[0124] Step 5: Vulcanization in vulcanization tank: put the rubber roller obtained in the fourth step into the vulcanization tank, close the tank door, introduce steam into the vulcanization tank and vulcanize by gradually increasing the temperature in steps and keeping the temperature for a long time. While introducing steam, open the compressed air valve and introduce compressed air to make the pressure in the vulcanization tank reach 0.45MPa within 0.5hr;
[0125] The procedure for step-by-step heating and heat preservation for long-term heating vulcanization is as follows: first, heat to 90°C and keep at 90°C for 1 hour; then heat to 100°C and keep at 100°C for 1 hour; then heat to 130°C and keep at 130°C for 1 hour; then heat to 150°C and keep at 150°C for 6 hours; during the entire heating vulcanization process, the pressure in the vulcanization tank is maintained at 0.45MPa.
[0126] Step 6: Turning and grinding: The rubber roller vulcanized in the fifth step is naturally cooled to room temperature indoors, processed with a PCD rubber turning tool, and then fine-processed with a special grinder.
[0127] Example 6
[0128] This embodiment provides the application of the rubber roller in Example 4. The product corresponding to the above-mentioned rubber roller: D350*D310*1500 model rubber roller is used in an Anhui enterprise to apply paint to the surface of oriented silicon steel to form a coating. The rubber roller can be used for 7 days at a time and can be reused 10 times.
[0129] The above content is a schematic description of the present invention and its implementation methods, which is not restrictive. What is shown in the embodiment is only one of the implementation methods of the present invention, and the actual implementation method is not limited thereto. Therefore, if a person of ordinary skill in the art is inspired by it and designs implementation methods and embodiments similar to the technical solution without creative design without departing from the purpose of the invention, they should all fall within the scope of protection of the present invention.
Claims
1. A rubber material for coating oriented silicon steel, characterized in that: The rubber compound is used to apply a coating to the surface of the oriented silicon steel to form a coating. The rubber compound comprises the following raw material components calculated by weight: Nitrile rubber: 50-55 parts; Carbon black: 20-25 parts; Zinc oxide: 1-10 parts; Stearic acid: 0.5-1 part; Plasticizer: 1.5-5.5 parts; Polyethylene glycol: 1.5-2.5 parts; Tackifier: 1.5-2.3 parts; Inorganic filler: 5.4-10.6 parts; Wear-resistant resin: 4-10.6 parts; Vulcanizing agent: 0.5-2.1 parts; Accelerator: 0.25-1.8 parts; Anti-scorching agent: 0.5-1 part.
2. The rubber material for coating oriented silicon steel according to claim 1, characterized in that: The plasticizer includes one or more of petroleum plasticizer, coal tar plasticizer, pine tar plasticizer, fat plasticizer and synthetic plasticizer.
3. The rubber material for coating oriented silicon steel according to claim 2, characterized in that: The tackifier includes one or more of terpene resin C5 and terpene resin C9.
4. The rubber material for coating oriented silicon steel according to claim 3, characterized in that: The inorganic filler includes one or more of zinc oxide, magnesium oxide, white carbon black and titanium dioxide.
5. The rubber material for coating oriented silicon steel according to claim 4, characterized in that: The wear-resistant resin includes one or more of epoxy resin, phenolic resin and acrylic resin.
6. The rubber material for coating oriented silicon steel according to claim 5, characterized in that: The vulcanizing agent includes one or more of an elemental sulfur vulcanizing agent, a sulfur donor vulcanizing agent, a peroxide vulcanizing agent, a metal oxide vulcanizing agent, a quinone derivative resin vulcanizing agent, and an amine compound vulcanizing agent.
7. The rubber material for coating oriented silicon steel according to claim 6, characterized in that: The accelerator includes: accelerator CZ: 0.15-0.9 parts; accelerator DTDM: 0.1-0.9 parts; The anti-scorching agent includes one or more of an organic acid anti-scorching agent, a nitroso compound anti-scorching agent and a sulfonamide anti-scorching agent.
8. The rubber material for coating oriented silicon steel according to any one of claims 1 to 7, characterized in that: The hardness Shore A of the rubber material is 61 to 63 degrees.
9. A rubber roller, characterized in that: The rubber roller comprises a roller core and the rubber material according to any one of claims 1 to 8, and the rubber material covers the roller core.
10. The method for preparing a rubber roller according to claim 9, characterized in that: The following steps are involved: S1. Banburying: After plasticizing the nitrile rubber, carbon black, inorganic filler, zinc oxide, stearic acid, polyethylene glycol, wear-resistant resin and tackifier are added and mixed, and then the plasticizer is added and mixed, the plug is lifted, the rubber is discharged, and the mixing is stopped to obtain a masterbatch after banburying; S2. Filtration: The masterbatch after mixing is filtered using UTH filtration technology to obtain a filtered masterbatch; S3. Sulfur refining: The filtered masterbatch is placed on the roller of the mixing mill, and the compounding agents are added: sulfur, accelerator, scorch retarder, and the compounding agents are all eaten into the masterbatch and then the knife is turned over and the rubber is finally obtained by sheeting; S4. Wrapping and rubber coating: coating the roller core with the rubber material to obtain a rubber roller; S5. Vulcanization in an autoclave: The rubber roller coated in step S4 is sent to an autoclave for vulcanization; S6. Turning and grinding: After the rubber roller vulcanized in step S5 is cooled to room temperature, it is subjected to turning and grinding.
Citation Information
Patent Citations
Butyronitrile rubber roller manufacturing method
CN1066023A
Glue material for coating rubber roller, coating rubber roller and preparation method of coating rubber roller
CN108264662A
Mixed rubber stock for rubber pad of air-conditioning compressor and preparation method thereof
CN109021315A