Water glass air-drying coating for cast steel and preparation method of water glass air-drying coating
By combining modified water glass with modified polyurethane resin and adding raw materials such as zirconium powder, an environmentally friendly self-drying coating for cast steel water glass is prepared, which solves the toxic substances and corrosion problems in existing cast steel coatings and achieves efficient Steel protection and environmental protection performance.
Patent Information
- Application Number
- CN202411012167.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-08
AI Technical Summary
The sodium chloride used in existing cast steel coatings is toxic, endangering the environment and human health, and failing to effectively prevent steel corrosion, resulting in serious steel losses and hindering the development of the industrial economy.
Modified water glass is combined with modified polyurethane resin, and raw materials such as zirconium powder, sepiolite powder and sodium dodecyl sulfate are added. Through strict control of the synthesis process, an environmentally friendly self-drying coating for cast steel water glass is prepared to improve the Mechanical properties and corrosion resistance of the coating.
The water-drying self-drying coating for cast steel is environmentally friendly and pollution-free, with a fast drying speed. The coating formed has a good protective effect, which significantly improves the corrosion resistance and comprehensive performance of steel and reduces the emission of harmful substances.
Smart Images

Figure BDA0004964702930000091 
Figure BDA0004964702930000101
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of coating processing, and in particular relates to a water glass self-drying coating for cast steel and a preparation method thereof. Background Art
[0002] Casting coatings are casting auxiliary materials that cover the surface of the core during the casting process to improve its surface fire resistance, chemical stability, resistance to metal liquid erosion, and resistance to sand adhesion. Before being applied to the surface of the sand mold and sand core, the casting coating is a colloidal physical suspension dispersion system. This physical suspension dispersion system usually contains refractory powder, carrier, suspending agent, binder and additives, etc. Among them, the refractory powder is the basis of the coating. It is suspended in the coating with the help of the suspending agent and is evenly coated on the working surface of the casting core during casting. After the carrier liquid evaporates, the binder dries the powder into a dense coating to protect the working surface. Therefore, it is widely used in casting production. With the development of casting mold types and casting alloy types, casting coatings are also diversified.
[0003] Patent CN 117844282 A discloses a cast steel coating for modified water glass sand and its processing technology. The components of the cast steel coating in the invention are: zirconium powder, resin, lithium-based bentonite, additives, organic bentonite, alcohol and water; wherein the additive is a mixture of sodium dodecylbenzene sulfonate, n-butanol and sodium chlorophenol. The invention adopts relatively common materials to solve the defects of sand sticking to cast steel parts and the unsightly surface of castings, reduce the amount of post-processing grinding, reduce waste, improve efficiency and reduce costs; improve the fire resistance of the coating, low cost price, significantly reduce the sand sticking defects of castings, save cleaning and grinding time, and significantly improve the appearance quality. However, the sodium chlorophenol used in the cast steel coating is toxic and seriously endangers the environment and human health. Moreover, the performance test data of the cast steel coating is not disclosed in the patent, and it has no practical reference significance.
[0004] In addition, according to reports, the total amount of steel scrapped due to corrosion in the world each year can reach one-tenth of the total steel production. The large amount of steel loss has seriously hindered the development of industrial economy. The role of cast steel coating is to protect steel from the influence of corrosive environment, shield the penetration of corrosive media, extend the service life of steel, and indirectly promote the development of industrial economy. On the one hand, cast steel coating with excellent performance requires to reduce the emission of harmful substances as much as possible, and on the other hand, its coating performance is required to effectively prevent the occurrence of steel corrosion. Therefore, the research and development of new environmentally friendly cast steel coatings is both a challenge and an opportunity for researchers from various countries, and is of great significance to the development of industry. Summary of the invention
[0005] The invention discloses a self-drying water glass coating for cast steel and a preparation method thereof. The preparation process is simple and easy to operate. The self-drying water glass coating for cast steel is environmentally friendly and pollution-free, has a fast drying speed, and the formed coating has a good protective effect on steel and can effectively prevent the occurrence of corrosion problems.
[0006] The first aspect of the present invention provides a self-drying water glass coating for cast steel, which comprises the following raw materials by mass percentage:
[0007] Zirconium powder 40%-55%, modified polyurethane resin 5%-10%, modified water glass 1%-1.5%, sepiolite powder 0.8%-1.1%, sodium lauryl sulfate 0.7%-1.2%, organic bentonite 0.7%-1.3%, ethylene glycol 5%-6.5%, water 40%-60%.
[0008] The water glass self-drying coating provided by the present invention is environmentally friendly and pollution-free, has good comprehensive performance, and has a good protective effect on steel. The present invention uses modified water glass with good thermal stability, durability, adhesion, wear resistance and fast drying speed and synthetic modified polyurethane resin in the self-drying coating for cast steel. The two can produce a synergistic effect, significantly improving the mechanical properties and corrosion resistance of the self-drying coating for cast steel, and the present invention selects zirconium powder as a refractory powder to improve the density, strength and high temperature resistance of the coating; selects sepiolite powder as a suspending agent to avoid the problem of precipitation of the coating and being unfavorable for brushing; selects sodium dodecyl sulfate as a surfactant to reduce surface tension and improve the wettability of the coating; selects organic bentonite as a stabilizer and thickener, so that the coating has good suspension stability, high temperature stability, water resistance and chemical stability.
[0009] In some embodiments, the preparation steps of the modified polyurethane resin are:
[0010] (1) adding a silane coupling agent to the polyacrylonitrile hollow microsphere emulsion, stirring and reacting at 50-60° C. for 20-24 hours to obtain a modified polyacrylonitrile hollow microsphere emulsion;
[0011] (2) Evenly mixing polyester polyol, double-terminal hydroxypropyl silicone oil and polyisocyanate, adding stannous octoate, reacting at 80-90° C. for 2-3 hours, cooling to 30-40° C., adding dimethylolpropionic acid and 1,4-butanediol to the system, reacting at 75-85° C. for 3-4 hours, cooling to 30-40° C., adding triethylamine for neutralization for 20-30 minutes, and obtaining a polyurethane prepolymer;
[0012] (3) Adding the modified polyacrylonitrile hollow microsphere emulsion obtained in step (1) to the polyurethane prepolymer of step (2), stirring for 20-30 minutes, and then dropping ethylenediamine thereinto, stirring evenly, to obtain a modified polyurethane resin.
[0013] In some embodiments, the mass ratio of the polyacrylonitrile hollow microsphere emulsion to the silane coupling agent in step (1) is (18-20):1.
[0014] Preferably, in step (1), the mass ratio of the polyacrylonitrile hollow microsphere emulsion to the silane coupling agent is 19:1.
[0015] Further preferably, the silane coupling agent is KH550.
[0016] In some embodiments, the molar ratio of the polyester polyol, the double-terminal hydroxypropyl silicone oil and the polyisocyanate in step (2) is 1:(5-6):(13-15); the polyester polyol is an aliphatic polyester polyol with an average molecular weight of 1000-2000.
[0017] Preferably, in the step (2), the molar ratio of the polyester polyol, the double-terminal hydroxypropyl silicone oil and the polyisocyanate is 1:5.5:14; and the polyester polyol is poly(1,4-butylene adipate) polyol with an average molecular weight of 2000.
[0018] In some embodiments, the amount of the modified polyacrylonitrile hollow microsphere emulsion used in step (3) is 3.5-5 wt % of the polyurethane prepolymer.
[0019] Preferably, the mass of the modified polyacrylonitrile hollow microsphere emulsion in step (3) is 4.5wt% of the polyurethane prepolymer.
[0020] Preferably, the preparation method of the polyacrylonitrile hollow microsphere emulsion refers to patent CN 110408313 A.
[0021] The present invention synthesizes a polyurethane prepolymer by strictly controlling the synthesis process from a certain molar ratio of polyester polyol, double-terminal hydroxypropyl silicone oil and polyisocyanate, and introduces a polyacrylonitrile hollow microsphere emulsion modified by a silane coupling agent therein to obtain a modified polyurethane resin, and the resin is applied to a water glass self-drying coating, which can significantly improve the comprehensive performance of the coating. This is because, in the present invention, by controlling the molar ratio of polyester polyol, double-terminal hydroxypropyl silicone oil and polyisocyanate, the synthesized polyurethane prepolymer has a certain content of hard segment and soft segment, and the functional group of the polyurethane prepolymer can be grafted to the surface of the polyacrylonitrile hollow microsphere to form a highly stable resin system; on the other hand, the present invention uses KH550 to modify the polyacrylonitrile hollow microsphere emulsion, so that the surface of the polyacrylonitrile hollow microsphere is rich in amino groups, the thermal stability of the polyacrylonitrile hollow microsphere emulsion is improved, and its compatibility with other substances in the coating system is improved, which is conducive to improving the comprehensive performance of the water glass self-drying coating.
[0022] In some embodiments, the preparation steps of the modified water glass are:
[0023] Add calcium oxide to water glass, stir while adding, let stand for 10-20 minutes after mixing evenly, centrifuge, add silane coupling agent, polypropylene glycol and defoaming agent to the supernatant obtained after centrifugation, stir evenly, and obtain modified water glass.
[0024] In some embodiments, the mass ratio of calcium oxide to the volume of water glass is 1 g: (8-10) mL.
[0025] Preferably, the mass ratio of the calcium oxide to the volume of water glass is 1 g:9 mL.
[0026] In some embodiments, the mass ratio of the supernatant, the silane coupling agent, the polypropylene glycol and the defoaming agent is (47-52):(2-3):(1.5-2.5):1.
[0027] Preferably, the mass ratio of the supernatant, the silane coupling agent, the polypropylene glycol and the defoaming agent is 50:2.5:2:1.
[0028] The applicant has found that the use of calcium oxide to modify water glass, and adding a certain amount of silane coupling agent, polypropylene glycol and defoaming agent, and applying it to the coating can improve the stability of the self-drying coating and accelerate the drying speed of the coating. This is because, on the one hand, calcium oxide can react with the free water in the water glass to generate calcium hydroxide, which concentrates the water glass, increases the pH value, and slows down the polymerization of silicon-oxygen polymers in the water glass; on the other hand, the generated calcium hydroxide dissociates calcium ions, which synergize with the increased pH value of the water glass, so that the silicon-oxygen polymer exists mainly in the form of chain polymers, forming a stronger calcium silicate hydrate gel, thereby improving the mechanical strength and water resistance of the water glass. At the same time, silane coupling agent, polypropylene glycol and defoamer are added to water glass. The silane coupling agent in the modified water glass can react with raw materials such as silicate and modified polyurethane resin in the system to form a bond, forming a chemical bond connection between the two phase interfaces, effectively improving the mechanical properties of the material; polypropylene glycol can improve the thermal stability, durability, adhesion, wear resistance and drying speed of the coating, and improve the fluidity and coating performance of the coating. The defoamer can eliminate bubbles caused by stirring during the preparation process and improve the wettability of the coating.
[0029] In some embodiments, the zirconium powder has an average particle size ranging from 40 to 80 μm.
[0030] Preferably, the average particle size of the zirconium powder is 60 μm.
[0031] Zirconium powder has high melting temperature, strong corrosion resistance, good thermal shock resistance and high chemical stability. In the present invention, zirconium powder with a certain particle size is added to the coating system as refractory powder, which can be well dispersed and suspended in the coating system, which is beneficial to improving the corrosion resistance and thermal stability of the water glass self-drying coating.
[0032] A second aspect of the present invention provides a method for preparing a self-drying water glass coating for cast steel, comprising the following preparation steps:
[0033] S1, add sepiolite powder and organic bentonite to water, stir evenly, let stand for 1-2 days, then add zirconium powder and sodium dodecyl sulfate and stir for 9-20 hours to obtain paste 1;
[0034] S2, adding ethylene glycol and modified water glass to the modified polyurethane resin, stirring for 10-20 hours, to obtain paste 2;
[0035] S3, the paste 1 obtained in step S1 and the paste 2 obtained in step S2 are mixed evenly to obtain a self-drying water glass coating for cast steel.
[0036] Compared with the prior art, the present invention has the following beneficial effects:
[0037] 1. The present invention uses modified water glass and synthetic modified polyurethane resin together in the self-drying coating for cast steel, and the two can significantly improve the mechanical properties and corrosion resistance of the self-drying coating for cast steel, and is used together with zirconium powder, sepiolite powder, sodium dodecyl sulfate and organic bentonite to obtain an environmentally friendly and pollution-free water glass self-drying coating with good comprehensive performance.
[0038] 2. The present invention synthesizes a polyurethane resin from polyester polyol, double-terminal hydroxypropyl silicone oil and polyisocyanate by strictly controlling the synthesis process, and introduces a polyacrylonitrile hollow microsphere emulsion modified by a silane coupling agent therein to obtain a modified polyurethane resin. The resin is applied to a water glass self-drying paint, which can significantly improve the comprehensive performance of the paint.
[0039] 3. The present invention uses calcium oxide to modify water glass, and adds a certain amount of silane coupling agent, polypropylene glycol and defoaming agent. The obtained modified water glass has high mechanical strength and water resistance. Applying it to coatings can improve the mechanical properties of the coatings and accelerate the drying speed of the coatings. DETAILED DESCRIPTION
[0040] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0041] In order to better illustrate the specific implementation mode of the present invention, further examples are given below.
[0042] The polyacrylonitrile hollow microsphere emulsion used in the present invention is obtained by referring to Example 1 in patent CN 110408313 A; the silane coupling agent used is KH550; the polyester polyol used is poly(1,4-butylene adipate) polyol with an average molecular weight of 2000, purchased from Jining Liduo Chemical Co., Ltd.; the double-terminal hydroxypropyl silicone oil used is double-terminal hydroxypropyl silicone oil IOTA2030-20, purchased from Anhui Aiyota Silicone Oil Co., Ltd.; the polyisocyanate used is isophorone diisocyanate, purchased from Shandong Jiaying Chemical Technology Co., Ltd.; the average molecular weight of the polypropylene glycol used is 1,4-butylene adipate polyol with an average molecular weight of 2000, purchased from Jining Liduo Chemical Co., Ltd. The molecular weight is 2000, purchased from Guangzhou Ya Chuangxin Materials Co., Ltd.; the defoamer used is defoamer DF-831, purchased from Dongguan Defeng Defoamer Co., Ltd.; the average particle size of the zirconium powder used is 60μm, purchased from Hunan Fujia Technology Co., Ltd.; the sepiolite powder used is sepiolite powder with item number 200m purchased from Nanyang Wolong District Leibao Sepiolite Processing Co., Ltd.; the organic bentonite used is organic bentonite HW-100, purchased from Shandong Huawei Bentonite Co., Ltd.
[0043] Preparation Example 1
[0044] The preparation steps of modified polyurethane resin are:
[0045] (1) adding 5 g of silane coupling agent to 95 g of polyacrylonitrile hollow microsphere emulsion, stirring and reacting at 55° C. for 22 h to obtain a modified polyacrylonitrile hollow microsphere emulsion;
[0046] (2) 0.1 mol of polyester polyol, 0.55 mol of double-terminal hydroxypropyl silicone oil and 1.4 mol of polyisocyanate were uniformly mixed, 0.04 g of stannous octoate was added, and the mixture was reacted at 85° C. for 2.5 h, and then cooled to 35° C., and then 0.2 mol of dimethylolpropionic acid and 0.65 mol of 1,4-butanediol were added to the system, and the mixture was reacted at 80° C. for 3.5 h, and then cooled to 35° C., and 0.25 mol of triethylamine was added for neutralization for 25 min to obtain a polyurethane prepolymer;
[0047] (3) Add 4.5 g of the modified polyacrylonitrile hollow microsphere emulsion obtained in step (1) to 100 g of the polyurethane prepolymer obtained in step (2), stir for 25 min, then dropwise add 10 mL of a 3 mol / L aqueous solution of ethylenediamine, stir evenly, and obtain a modified polyurethane resin.
[0048] Preparation Example 2
[0049] The preparation steps of modified polyurethane resin are:
[0050] (1) 0.1 mol of polyester polyol, 0.55 mol of double-terminal hydroxypropyl silicone oil and 1.4 mol of polyisocyanate were uniformly mixed, 0.04 g of stannous octoate was added, and the mixture was reacted at 85° C. for 2.5 h, and then cooled to 35° C., and then 0.2 mol of dimethylol propionic acid and 0.65 mol of 1,4-butanediol were added to the system, and the mixture was reacted at 80° C. for 3.5 h, and then cooled to 35° C., and 0.25 mol of triethylamine was added for neutralization for 25 min to obtain a polyurethane prepolymer;
[0051] (2) Add 4.5 g of polyacrylonitrile hollow microsphere emulsion to 100 g of the polyurethane prepolymer of step (2), stir for 25 min, then dropwise add 10 mL of 3 mol / L ethylenediamine aqueous solution, stir evenly, to obtain a modified polyurethane resin.
[0052] Preparation Example 3
[0053] The preparation steps of polyurethane resin are:
[0054] (1) 0.1 mol of polyester polyol, 0.55 mol of double-terminal hydroxypropyl silicone oil and 1.4 mol of polyisocyanate were uniformly mixed, 0.04 g of stannous octoate was added, and the mixture was reacted at 85° C. for 2.5 h, and then cooled to 35° C., and then 0.2 mol of dimethylol propionic acid and 0.65 mol of 1,4-butanediol were added to the system, and the mixture was reacted at 80° C. for 3.5 h, and then cooled to 35° C., and 0.25 mol of triethylamine was added for neutralization for 25 min to obtain a polyurethane prepolymer;
[0055] (2) Add 10 mL of a 3 mol / L aqueous solution of ethylenediamine to 100 g of the polyurethane prepolymer prepared in step (2), and stir evenly to obtain a polyurethane resin.
[0056] Preparation Example 4
[0057] The preparation steps of the modified polyurethane resin are the same as those in Preparation Example 1, except that 3 g of silane coupling agent is used in step (1).
[0058] Preparation Example 5
[0059] The preparation steps of the modified polyurethane resin are the same as those in Preparation Example 1, except that the amount of the double-terminal hydroxypropyl silicone oil used in step (2) is 0.4 mol.
[0060] Preparation Example 6
[0061] The preparation steps of the modified polyurethane resin are the same as those in Preparation Example 1, except that the polyisocyanate used in step (2) is 1 mol.
[0062] Preparation Example 7
[0063] The preparation steps of modified water glass are:
[0064] At a stirring speed of 150 r / min, add 20 g of calcium oxide to 180 mL of water glass, mix well, let stand for 15 min, and centrifuge at 1000 r / min. Add 5 g of silane coupling agent, 4 g of polypropylene glycol and 2 g of defoaming agent to the supernatant obtained after 100 g centrifugation, stir well, and obtain modified water glass.
[0065] Preparation Example 8
[0066] The preparation steps of modified water glass are:
[0067] Add 5 g of silane coupling agent, 4 g of polypropylene glycol and 2 g of defoaming agent to 100 g of water glass, stir evenly to obtain modified water glass.
[0068] Preparation Example 9
[0069] The preparation steps of modified water glass are the same as those in Preparation Example 7, except that 10 g of calcium oxide is used.
[0070] Preparation Example 10
[0071] The preparation steps of the modified water glass are the same as those of Preparation Example 7, except that no silane coupling agent is added.
[0072] Example 1
[0073] A method for preparing a self-drying water glass coating for cast steel comprises the following steps:
[0074] S1, add 8 g of sepiolite powder and 7 g of organic bentonite to 400 g of water, stir evenly, let stand for 1 day, then add 400 g of zirconium powder and 7 g of sodium dodecyl sulfate, stir at 200 r / min for 9 h, and obtain paste 1;
[0075] S2, adding 50 g of ethylene glycol and 10 g of modified water glass to 50 g of modified polyurethane resin, stirring for 10 h, to obtain paste 2;
[0076] S3, the paste 1 obtained in step S1 and the paste 2 obtained in step S2 are mixed evenly to obtain a self-drying water glass coating for cast steel.
[0077] The modified polyurethane resin used is obtained from Preparation Example 1; the modified water glass used is obtained from Preparation Example 7.
[0078] Example 2
[0079] A method for preparing a self-drying water glass coating for cast steel comprises the following steps:
[0080] S1, add 11g of sepiolite powder and 13g of organic bentonite to 600g of water, stir evenly, let stand for 2 days, then add 550g of zirconium powder and 12g of sodium dodecyl sulfate, stir at 200r / min for 20h, and obtain paste 1;
[0081] S2, adding 65 g of ethylene glycol and 15 g of modified water glass to 100 g of modified polyurethane resin, stirring for 20 h, to obtain paste 2;
[0082] S3, the paste 1 obtained in step S1 and the paste 2 obtained in step S2 are mixed evenly to obtain a self-drying water glass coating for cast steel.
[0083] The modified polyurethane resin used is obtained from Preparation Example 1; the modified water glass used is obtained from Preparation Example 7.
[0084] Example 3
[0085] A method for preparing a self-drying water glass coating for cast steel comprises the following steps:
[0086] S1, add 10g of sepiolite powder and 10g of organic bentonite to 500g of water, stir evenly, let stand for 1.5 days, then add 500g of zirconium powder and 10g of sodium dodecyl sulfate, stir at 200r / min for 15h, and obtain paste 1;
[0087] S2, adding 60 g of ethylene glycol and 13 g of modified water glass to 80 g of modified polyurethane resin, stirring for 15 h, to obtain paste 2;
[0088] S3, the paste 1 obtained in step S1 and the paste 2 obtained in step S2 are mixed evenly to obtain a self-drying water glass coating for cast steel.
[0089] The modified polyurethane resin used is obtained from Preparation Example 1; the modified water glass used is obtained from Preparation Example 7.
[0090] Example 4
[0091] A method for preparing a self-drying water glass coating for cast steel, the specific implementation method is the same as that of Example 3, except that the modified polyurethane resin used is obtained from Preparation Example 2.
[0092] Example 5
[0093] A method for preparing a self-drying water glass coating for cast steel, the specific implementation method is the same as that of Example 3, except that the modified polyurethane resin used is obtained from Preparation Example 4.
[0094] Example 6
[0095] A method for preparing a self-drying water glass coating for cast steel, the specific implementation method is the same as that of Example 3, except that the modified polyurethane resin used is obtained from Preparation Example 5.
[0096] Example 7
[0097] A method for preparing a self-drying water glass coating for cast steel, the specific implementation method is the same as that of Example 3, except that the modified polyurethane resin used is obtained from Preparation Example 6.
[0098] Example 8
[0099] A method for preparing a self-drying water glass coating for cast steel, the specific implementation method is the same as that of Example 3, except that the modified water glass used is obtained from Preparation Example 8.
[0100] Example 9
[0101] A method for preparing a self-drying water glass coating for cast steel, the specific implementation method is the same as that of Example 3, except that the modified water glass used is obtained from Preparation Example 9.
[0102] Example 10
[0103] A method for preparing a self-drying water glass coating for cast steel, the specific implementation method is the same as that of Example 3, except that the modified water glass used is obtained from Preparation Example 10.
[0104] Comparative Example 1
[0105] A method for preparing a self-drying water glass coating for cast steel, wherein the specific implementation method is the same as that of Example 3, except that the polyurethane resin of Preparation Example 3 of equal mass is used to replace the modified polyurethane resin.
[0106] Comparative Example 2
[0107] A method for preparing a self-drying water glass coating for cast steel, wherein the specific implementation method is the same as that of Example 3, except that unmodified water glass of equal mass is used instead of modified water glass.
[0108] Performance test of water glass self-drying paint
[0109] The viscosity, suspension rate, gas evolution, wear resistance, coating appearance after coating, drying and cooling and high-temperature explosion crack grade of the water glass self-drying coating obtained in Examples 1-10 and Comparative Examples 1-2 were tested. The test method was strictly carried out in accordance with JB / T9226-2008 standard. The specific test results are shown in Table 1.
[0110] Table 1
[0111]
[0112]
[0113] It can be seen from Table 1 that the water glass self-drying coatings prepared in Examples 1-3 have good performance, moderate viscosity, high suspension rate, low gas evolution, and good wear resistance. After coating, drying and cooling, the coating has no cracks or pinholes, and the high-temperature explosion crack level is the highest, which indirectly reflects that the corrosion resistance of the water glass self-drying coating is also good.
[0114] Compared with Example 3, the preparation process of the modified polyurethane resin used in Examples 4-7 was changed (polyacrylonitrile hollow microsphere emulsion not modified by silane coupling agent, polyacrylonitrile hollow microsphere emulsion modified by a small amount of silane coupling agent, and raw material ratio), so that the thermal stability of the polyacrylonitrile hollow microsphere emulsion and the compatibility with other substances in the system decreased, and the content of the soft segment and the hard segment in the modified polyurethane resin changed, resulting in a decrease in the comprehensive performance of the water glass self-drying coating; the polyurethane resin used in Comparative Example 1 did not add polyacrylonitrile hollow microsphere emulsion, and compared with the modified polyurethane resin used in Example 3, its thermal stability and wear resistance were worse, so that the coating had cracks and pinholes, and the high-temperature explosion cracking grade was also reduced.
[0115] Compared with Example 3, calcium oxide is not added to the modified water glass used in Example 8, and the silicon and oxygen in the water glass cannot be polymerized to form a high-strength hydrated calcium silicate gel, which further affects the mechanical strength and water resistance of the water glass, and reduces the performance of the water glass self-drying coating; in Example 9, the amount of calcium oxide added to the modified water glass used is changed, and the mechanical strength and water resistance of the modified water glass are deteriorated, so that the performance of the water glass self-drying coating is also reduced; in Example 10, no silane coupling agent is added to the modified water glass used, so that the modified water glass cannot react with the raw materials such as silicate and modified polyurethane resin in the system to form a bond, which weakens the performance of the water glass self-drying coating; in Comparative Example 2, unmodified water glass is used instead of modified water glass, and the comprehensive performance of the unmodified water glass is poor, which reduces the comprehensive performance of the water glass self-drying coating.
[0116] The above is only a preferred embodiment of the present invention and does not constitute any form of limitation to the present application. Although the present application is disclosed as above in the preferred embodiment, it is not intended to limit the present application. Any technician familiar with the profession, without departing from the scope of the technical solution of the present application, using the technical content disclosed above to make slight changes or modifications are equivalent to equivalent implementation cases. However, any simple modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention are still within the scope of the technical solution.
Claims
1. A self-drying water glass coating for cast steel, characterized in that: In terms of mass percentage, it includes the following raw materials: Zirconium powder 40%-55%, modified polyurethane resin 5%-10%, modified water glass 1%-1.5%, sepiolite powder 0.8%-1.1%, sodium lauryl sulfate 0.7%-1.2%, organic bentonite 0.7%-1.3%, ethylene glycol 5%-6.5%, water 40%-60%.
2. A self-drying water glass coating for cast steel according to claim 1, characterized in that: The preparation steps of the modified polyurethane resin are: (1) adding a silane coupling agent to the polyacrylonitrile hollow microsphere emulsion, stirring and reacting at 50-60° C. for 20-24 hours to obtain a modified polyacrylonitrile hollow microsphere emulsion; (2) Evenly mixing polyester polyol, double-terminal hydroxypropyl silicone oil and polyisocyanate, adding stannous octoate, reacting at 80-90° C. for 2-3 hours, cooling to 30-40° C., adding dimethylolpropionic acid and 1,4-butanediol to the system, reacting at 75-85° C. for 3-4 hours, cooling to 30-40° C., adding triethylamine for neutralization for 20-30 minutes, and obtaining a polyurethane prepolymer; (3) Adding the modified polyacrylonitrile hollow microsphere emulsion obtained in step (1) to the polyurethane prepolymer of step (2), stirring for 20-30 minutes, and then dropping ethylenediamine thereinto, stirring evenly, to obtain a modified polyurethane resin.
3. A self-drying water glass coating for cast steel according to claim 2, characterized in that: In the step (1), the mass ratio of the polyacrylonitrile hollow microsphere emulsion to the silane coupling agent is (18-20):
1.
4. A self-drying water glass coating for cast steel according to claim 2, characterized in that: In the step (2), the molar ratio of polyester polyol, double-terminal hydroxypropyl silicone oil and polyisocyanate is 1:(5-6):(13-15); the polyester polyol is an aliphatic polyester polyol with an average molecular weight of 1000-2000.
5. A self-drying water glass coating for cast steel according to claim 2, characterized in that: The amount of the modified polyacrylonitrile hollow microsphere emulsion used in step (3) is 3.5-5wt% of the polyurethane prepolymer.
6. A self-drying water glass coating for cast steel according to claim 1, characterized in that: The preparation steps of the modified water glass are: Add calcium oxide to water glass, stir while adding, let stand for 10-20 minutes after mixing evenly, centrifuge, add silane coupling agent, polypropylene glycol and defoaming agent to the supernatant obtained after centrifugation, stir evenly, and obtain modified water glass.
7. A self-drying water glass coating for cast steel according to claim 6, characterized in that: The mass ratio of the calcium oxide to the volume of water glass is 1g:(8-10)mL.
8. A self-drying water glass coating for cast steel according to claim 7, characterized in that: The mass ratio of the supernatant, the silane coupling agent, the polypropylene glycol and the defoaming agent is (47-52):(2-3):(1.5-2.5):
1.
9. A self-drying water glass coating for cast steel according to claim 1, characterized in that: The average particle size of the zirconium powder is in the range of 40-80 μm.
10. A method for preparing a self-drying water glass coating for cast steel according to any one of claims 1 to 9, characterized in that: The method comprises the following preparation steps: S1, add sepiolite powder and organic bentonite to water, stir evenly, let stand for 1-2 days, then add zirconium powder and sodium dodecyl sulfate and stir for 9-20 hours to obtain paste 1; S2, adding ethylene glycol and modified water glass to the modified polyurethane resin, stirring for 10-20 hours, to obtain paste 2; S3, the paste 1 obtained in step S1 and the paste 2 obtained in step S2 are mixed evenly to obtain a self-drying water glass coating for cast steel.