Corrosion-resistant coating on surface of aluminum alloy and preparation method of corrosion-resistant coating

By preparing coatings of materials such as fluorinated polyurethane acrylate, antibacterially modified disulfide siloxane and nanotitanium dioxide on the surface of aluminum alloy, the rapid corrosion and biofilm formation problems of aluminum alloy surface in highly corrosive marine environments are solved. It achieves electrochemical resistance, anti-microbial corrosion and superhydrophobic effects.

CN118909537AInactive Publication Date: 2024-11-08TIANJIN CHENGDE METAL PRODUCTS CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411164526.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The surface of aluminum alloy is susceptible to active anions and microbial corrosion in highly corrosive marine environments, resulting in rapid corrosion and biofilm formation, thereby accelerating local corrosion.

Method used

A coating is made of fluorinated polyurethane acrylate, antibacterially modified disulfide silicone, nanotitanium dioxide and ethyl silicate, etc., and is prepared by spraying and calcining to form a dense corrosion-resistant coating with antibacterial and super Hydrophobic and anti-scaling properties.

Benefits of technology

It significantly improves the electrochemical and microbial corrosion resistance of the aluminum alloy surface, prevents the formation of biofilms, delays local corrosion, and is suitable for highly corrosive seawater environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005007444420000121
    Figure BDA0005007444420000121
Patent Text Reader

Abstract

The invention discloses a corrosion-resistant coating on an aluminum alloy surface and a preparation method of the corrosion-resistant coating, and relates to the technical field of non-ferrous metal surface treatment and corrosion prevention. The preparation method comprises the following steps: preparing siloxane containing disulfide bonds, grafting an antibacterial agent with mercaptan, and then preparing an antibacterial modified TiO2 nano core-shell material from siloxane and crystal growth type nano titanium dioxide; the preparation method comprises the following steps: preparing a SiO2 precursor solution, dropwise adding fluorinated polyurethane acrylate for in-situ polymerization, adding an antibacterial modified TiO2 nano core-shell material, and carrying out ultrasonic homogenization to obtain a coating; sequentially polishing the surface of an aluminum alloy test piece by using abrasive paper of 400-3000 meshes, ultrasonically cleaning and washing the aluminum alloy test piece, placing the aluminum alloy test piece in a dryer for later use, spraying the coating on the aluminum alloy test piece by using a spray gun, and calcining to obtain the corrosion-resistant coating on the aluminum alloy surface. The corrosion-resistant coating prepared by the method has the characteristics of electrochemical corrosion resistance, microbial corrosion resistance, scaling prevention and super-hydrophobicity, can be applied to a high-corrosion seawater environment, and is used for protecting an aluminum alloy matrix and the surface of the aluminum alloy matrix.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of nonferrous metal surface treatment and anti-corrosion, and in particular to a corrosion-resistant coating on the surface of an aluminum alloy and a preparation method thereof. Background Art

[0002] Aluminum alloys are widely used in aerospace, shipbuilding, automobile, construction, transportation, electronics and other fields due to their low density, strong thermal and electrical conductivity, machinability and good mechanical properties. When used in corrosive environments, especially in highly corrosive marine environments, the presence of certain active anions in the medium (such as Cl - ), these active anions are first adsorbed on the porous aluminum alloy matrix leaking out from the middle of the passivation film on the aluminum alloy surface which is not dense. The surface of the aluminum alloy matrix corrodes, making it activated, while the passivation film is still passive, thus forming an active-passive corrosion cell. Since the anode area is much smaller than the cathode area and the anode current density is very large, the corrosion develops deeply and the metal surface is quickly corroded into small holes. This phenomenon is called pitting corrosion.

[0003] In addition, since the oxide film formed naturally on the surface of aluminum alloy is loose, porous and hydrophilic, the aluminum alloy exposed to the corrosive environment without the protection of the oxide film attracts the floating microorganisms due to the electrostatic effect or van der Waals force. The microorganisms gradually "settle" on the surface of the aluminum alloy with holes, which fixes the anode area of ​​the corrosion cell and proliferates on the surface, secretes extracellular polymers, and forms a biofilm. The biofilm grows and thickens until it matures. Its composition is relatively complex, mainly a gel phase with a water content of more than 95%, composed of bacteria, extracellular polymers, corrosion products and suspended particles. The formation of the biofilm changes the electrostatic state and wetting properties of the metal surface, which is conducive to the aggregation and growth of bacteria and other microorganisms on the interface. With the maturity of the biofilm, the ion types and oxidation-reduction potential of the metal surface change sharply, and a pH gradient is formed in the membrane, and various mass transfer processes and complex chemical reactions occur successively. At the same time, bacteria gather together in the form of biofilms and cooperate with each other to make full use of the metabolic products of both parties to form an energy cycle, such as the cooperative relationship between a group of acid-producing bacteria and sulfate-reducing bacteria, and the symbiotic proliferation of aerobic and anaerobic bacteria. These microorganisms adhere together in the form of a consortium on the metal surface to work together, inducing the formation of biofilms and accelerating the microbial corrosion process: the established shielding layer blocks the mass transfer pathway of particles at the metal / solution interface, creating a unique corrosion microenvironment; forming a concentration cell; changing the structure of the inorganic passivation layer on the metal surface, promoting the removal of the protective film layer; affecting the redox state of the metal / solution interface. The formation of biofilms accelerates more severe local corrosion on the surface of aluminum alloys, including but not limited to pitting, crevice corrosion, and intergranular corrosion. Summary of the invention

[0004] The purpose of the present invention is to provide a corrosion-resistant coating for an aluminum alloy surface and a preparation method thereof, so as to solve the problems raised in the background technology, and to manufacture a coating for an aluminum alloy surface that is resistant to electrochemical and microbial corrosion, anti-scaling, and super-hydrophobic for use in a highly corrosive seawater environment.

[0005] To achieve the above object, the present invention provides the following technical solutions:

[0006] A corrosion-resistant coating on the surface of an aluminum alloy is obtained by coating, curing and drying a coating, wherein the coating comprises the following raw materials in parts by weight:

[0007] 40-60 parts of fluorinated polyurethane acrylate;

[0008] Antibacterial modified disulfide siloxane 0.4-0.6 parts;

[0009] Nano titanium dioxide 1.6-2.4 parts;

[0010] Ethyl silicate 37.38-56.07 parts;

[0011] 18-27 parts of ammonia water;

[0012] Anhydrous ethanol 79-118.5 parts;

[0013] 20-30 parts of deionized water.

[0014] Furthermore, the preparation steps of the fluorinated polyurethane acrylate are as follows:

[0015] 2 g of polyurethane acrylate and 0.2 g of triethyltriene were mixed in a homogeneous aqueous solution containing 3 mL of deionized water, 0.5 g of polytetrafluoroethylene and 20 μL of triethoxysilane were added dropwise to the aqueous solution, and then the mixture was magnetically stirred for 30 minutes to obtain fluorinated polyurethane acrylate.

[0016] It should be noted that triethoxysilane is chemically grafted with polyurethane acrylate, and polytetrafluoroethylene is physically cross-linked with polyurethane acrylate, and the combination of the two gives polyurethane acrylate fluorinated groups and high polymerization properties.

[0017] Furthermore, the preparation steps of the antibacterial modified disulfide siloxane are as follows:

[0018] Step 1: Mix vinyl triethoxysilane and 3,3′-dithiodipropionic acid, raise the temperature to 90°C and stir magnetically under a nitrogen atmosphere, raise the temperature to 150°C and react for 20 minutes when the mixed system becomes clear and transparent, lower the temperature to 45°C and continue the reaction when distillate is produced, stop the reaction when no distillate is produced, lower the temperature to room temperature, and evacuate for 30 minutes to obtain a yellow viscous disulfide bond-containing polysiloxane;

[0019] Step 2: Prepare PdCl 2 / dimethyl sulfoxide mixed solvent, the pH was adjusted to 4-5 with PBS buffer, pyrithione and the disulfide bond-containing polysiloxane prepared in step 1 were added, and homogenization was carried out at 80° C. for 2 h under a nitrogen atmosphere to prepare an antibacterial modified disulfide siloxane.

[0020] It should be noted that pyrithione and its salts are safe and environmentally friendly chemicals, widely used in shampoos and cosmetics. At the same time, it is also an antibacterial agent that destroys the bacterial cytoplasmic membrane, causing cell membrane dysfunction and ion leakage. It is a very effective inhibitor of sulfate-reducing bacteria sulfidation, which can inhibit the growth of sulfate-reducing bacteria and destroy their biofilm. The structure of pyrithione contains a pyridine ring, a thiol group, an oxygen ion and a sodium ion. The thiol group of pyrithione and disulfide-containing polysiloxane undergo a thiol-disulfide exchange reaction. Pyrithione is grafted onto the disulfide-containing polysiloxane as an asymmetric R group, providing antibacterial function for the coating and acting as a sustained-release antibacterial agent in actual application scenarios.

[0021] Furthermore, the mass ratio of vinyl triethoxysilane to 3,3′-dithiodipropionic acid in step 1 is 74.1:84.11.

[0022] Further, in step 1, PdCl 2 PdCl / DMSO mixed solvent 2 The concentration of PdCl is 0.025mmol / mL. 2 The usage ratio of the mixed solvent of / dimethyl sulfoxide, pyrithione and disulfide bond-containing polysiloxane is 2mL:0.5mmol:1mmol.

[0023] Furthermore, the nano titanium dioxide is a rutile titanium dioxide nanorod with a particle size of 50 nm; the purity of ethyl silicate is 99.9%; and the ammonia water is 27.3% ammonia water.

[0024] Furthermore, the coating preparation steps are as follows:

[0025] S1. 4 g of nano-titanium dioxide was uniformly dispersed in a mixture of 10 mL of deionized water and 10 mL of anhydrous ethanol by ultrasonic treatment. 250 μL of antibacterial modified disulfide siloxane was added to the nano-titanium dioxide dispersion, homogenized for 12 h, filtered, washed, and dried at 105 ° C for 6 h to obtain antibacterial modified TiO 2 Nano core-shell materials;

[0026] S2, deionized water, ammonia water and ethyl silicate were mixed in anhydrous ethanol under magnetic stirring for 20 minutes to obtain SiO 2 Precursor solution, add fluorinated polyurethane acrylate dropwise to SiO 2In-situ polymerization was carried out in the precursor solution for 12 h, and antibacterial modified TiO 2 The nano core-shell material is uniformly dispersed in the mixed solution through ultrasonic treatment to obtain a coating.

[0027] It should be noted that in order to reduce the encapsulation performance of the elastic fluorinated polyurethane acrylate, the inorganic phase SiO 2 Provided by a precursor formed by hydrolysis of tetraethyl orthosilicate.

[0028] Furthermore, in step S2, deionized water, ammonia water, ethyl silicate, anhydrous ethanol, fluorinated polyurethane acrylate and antibacterial modified TiO 2 The dosage ratio of the nano core-shell material is 10mL:10mL:20mL:50mL:20g:1g.

[0029] A method for preparing a corrosion-resistant coating on an aluminum alloy surface comprises the following steps:

[0030] (1) The surface of the aluminum alloy test piece with a thin plate structure was polished with 400, 600, 800, 1000, 1200, 2000 and 3000 mesh abrasive papers in sequence, and then ultrasonically cleaned in acetone for 5 minutes, rinsed with ethanol, and placed in a desiccator for standby use, thereby obtaining the aluminum alloy test piece after pretreatment;

[0031] (2) Use a spray gun to spray the coating onto the pre-treated aluminum alloy specimen at a pressure of 0.4-0.6 MPa, and calcine at 180° C. for 20 minutes to obtain a corrosion-resistant coating on the aluminum alloy surface.

[0032] It should be noted that the surface structure of the corrosion-resistant coating is a dense layered micro-nanostructure, which achieves excellent super-hydrophobicity and low surface energy modification. 2 The presence of nano-core-shell materials makes the rough structure of the corrosion-resistant coating surface relatively flat. This is because the long-crystalline rod-shaped nano-titanium dioxide is used in the preparation. 2 The whiskers have an inductive effect with a high aspect ratio, which greatly improves the leveling ability of the coating. 2 The nano core-shell material contains long-chain antibacterial modified disulfide siloxanes containing disulfide bonds. The siloxane stacking can be entangled with the fluorinated polyurethane acrylate resin to form a hierarchical network micro-nanostructure, which helps to give the corrosion-resistant coating superhydrophobicity. Due to the high hydrophobicity, extremely low surface energy and self-aggregation characteristics of the fluorinated group, the fluorinated fragments are more likely to aggregate on the coating surface, so the antibacterial modified TiO physically cross-linked with the fluorinated polyurethane acrylate resin 2 The nano core-shell material is partially accumulated on the surface of the corrosion-resistant coating. When the present invention is actually applied in a seawater environment rich in highly corrosive microorganisms, the pH of the seawater is alkaline, and the antibacterial modified TiO 2The disulfide bonds in the nano core-shell material will naturally decompose under alkaline conditions, releasing the bactericide pyridinethione into the micro-seawater ecosystem near the coating, killing a number of bacteria and algae represented by sulfate-reducing bacteria, and destroying the extracellular polymer biofilm secreted by the bacterial population, preventing the biofilm from accelerating more serious local corrosion on the aluminum alloy surface.

[0033] Compared with the prior art, the present invention has the following beneficial effects:

[0034] Preparation of antibacterial modified TiO 2 Nano core-shell material uses inductive effect long crystal rod-shaped nano titanium dioxide with high aspect ratio and high specific surface area as the core material to improve the leveling ability of the coating. Long-chain antibacterial modified disulfide siloxane containing disulfide bonds is prepared and used as the shell material and physically cross-linked with fluorinated polyurethane acrylate resin. The characteristics of the fluorinated group make the antibacterial modified TiO 2 The nano core-shell material is partially accumulated on the surface of the corrosion-resistant coating. When the present invention is actually applied in a seawater environment, the antibacterial modified TiO 2 The disulfide bonds in the nano core-shell material will naturally decompose under alkaline conditions, releasing bactericides to kill bacteria and algae such as sulfate-reducing bacteria and destroy the biofilm secreted by the bacterial population, preventing further microbial local corrosion.

[0035] The invention has the characteristics of resistance to electrochemical corrosion, resistance to microbial corrosion, anti-scaling and super-hydrophobicity, and can be used in a highly corrosive seawater environment to protect an aluminum alloy substrate and its surface. DETAILED DESCRIPTION

[0036] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solution of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0037] The preparation steps of fluorinated polyurethane acrylate are as follows:

[0038] 2 g of polyurethane acrylate and 0.2 g of triethyltriene were mixed in a homogeneous aqueous solution containing 3 mL of deionized water, 0.5 g of polytetrafluoroethylene and 20 μL of triethoxysilane were added dropwise to the aqueous solution, and then the mixture was magnetically stirred for 30 minutes to obtain fluorinated polyurethane acrylate.

[0039] The preparation steps of antibacterial modified disulfide siloxane are as follows:

[0040] Step 1: Mix 74.1 g of vinyl triethoxysilane and 84.11 g of 3,3′-dithiodipropionic acid, raise the temperature to 90° C. and stir magnetically under a nitrogen atmosphere. When the mixed system becomes clear and transparent, raise the temperature to 150° C. and react for 20 min. When distillate is produced, lower the temperature to 45° C. and continue the reaction until no distillate is produced. Stop the reaction, lower the temperature to room temperature, and evacuate for 30 min to obtain a yellow viscous disulfide bond-containing polysiloxane.

[0041] Step 2: Prepare 20 mL of PdCl 2 PdCl with a concentration of 0.025 mmol / mL 2 / dimethyl sulfoxide mixed solution, adjusted the pH to 4-5 with PBS buffer, added 0.8 mg of pyridinethione and 16.1 mg of disulfide-bonded polysiloxane, and homogenized at 50°C for 3 h to obtain antibacterial modified disulfide siloxane.

[0042] A method for preparing a corrosion-resistant coating on an aluminum alloy surface comprises the following steps:

[0043] (1) The surface of the aluminum alloy test piece with a thin plate structure was polished with 400, 600, 800, 1000, 1200, 2000 and 3000 mesh abrasive papers in sequence, and then ultrasonically cleaned in acetone for 5 minutes, rinsed with ethanol, and placed in a desiccator for standby use, thereby obtaining the aluminum alloy test piece after pretreatment;

[0044] (2) Use a spray gun to spray the coating onto the pre-treated aluminum alloy specimen at a pressure of 0.5 MPa, and calcine at 180° C. for 20 min to obtain a corrosion-resistant coating on the aluminum alloy surface.

[0045] Example 1

[0046] A corrosion-resistant coating on the surface of an aluminum alloy is obtained by coating, curing and drying the coating, wherein the coating comprises the following raw materials in parts by weight:

[0047] 50 parts of fluorinated polyurethane acrylate;

[0048] 0.5 parts of antibacterial modified disulfide siloxane;

[0049] 2 parts of nano titanium dioxide;

[0050] 46.73 parts of ethyl silicate;

[0051] 22.5 parts of ammonia water;

[0052] 98.8 parts of anhydrous ethanol;

[0053] 10 parts of deionized water.

[0054] The steps for preparing the coating are as follows:

[0055] S1. 4 g of nano-titanium dioxide was uniformly dispersed in a mixture of 10 mL of deionized water and 10 mL of anhydrous ethanol by ultrasonic treatment. 300 μL of antibacterial modified disulfide siloxane was added to the nano-titanium dioxide dispersion, homogenized for 12 h, filtered, washed, and dried at 105 ° C for 6 h to obtain antibacterial modified TiO 2 Nano core-shell materials.

[0056] S2, 1 mL of deionized water, 1 mL of ammonia water and 2 mL of ethyl silicate were mixed in 5 mL of anhydrous ethanol under magnetic stirring for 20 min to obtain SiO 2 Precursor solution, add fluorinated polyurethane acrylate dropwise to SiO 2 In-situ polymerization was carried out in the precursor solution for 12 h, and antibacterial modified TiO 2 The nano core-shell material is uniformly dispersed in the mixed solution through ultrasonic treatment to obtain a coating.

[0057] Example 2

[0058] A corrosion-resistant coating on the surface of an aluminum alloy is obtained by coating, curing and drying a coating, wherein the coating comprises the following raw materials in parts by weight:

[0059] 40 parts of fluorinated polyurethane acrylate;

[0060] 0.4 parts of antibacterial modified disulfide siloxane;

[0061] 1.6 parts of nano titanium dioxide;

[0062] 37.38 parts of ethyl silicate;

[0063] 18 parts of ammonia water;

[0064] Anhydrous ethanol 79 parts;

[0065] 20 parts of deionized water.

[0066] The steps for preparing the coating are as follows:

[0067] S1. 4 g of nano-titanium dioxide was uniformly dispersed in a mixture of 10 mL of deionized water and 10 mL of anhydrous ethanol by ultrasonic treatment. 300 μL of antibacterial modified disulfide siloxane was added to the nano-titanium dioxide dispersion, homogenized for 12 h, filtered, washed, and dried at 105 ° C for 6 h to obtain antibacterial modified TiO 2 Nano core-shell materials.

[0068] S2, 1 mL of deionized water, 1 mL of ammonia water and 2 mL of ethyl silicate were mixed in 5 mL of anhydrous ethanol under magnetic stirring for 20 min to obtain SiO 2 Precursor solution, add fluorinated polyurethane acrylate dropwise to SiO 2In-situ polymerization was carried out in the precursor solution for 12 h, and antibacterial modified TiO 2 The nano core-shell material is uniformly dispersed in the mixed solution through ultrasonic treatment to obtain a coating.

[0069] Example 3

[0070] A corrosion-resistant coating on the surface of an aluminum alloy is obtained by coating, curing and drying the coating, wherein the coating comprises the following raw materials in parts by weight:

[0071] 60 parts of fluorinated polyurethane acrylate;

[0072] 0.6 parts of antibacterial modified disulfide siloxane;

[0073] 2.4 parts of nano titanium dioxide;

[0074] Ethyl silicate 56.07 parts;

[0075] 27 parts of ammonia water;

[0076] 118.5 parts of anhydrous ethanol;

[0077] 30 parts of deionized water.

[0078] The steps for preparing the coating are as follows:

[0079] S1. 4 g of nano-titanium dioxide was uniformly dispersed in a mixture of 10 mL of deionized water and 10 mL of anhydrous ethanol by ultrasonic treatment. 300 μL of antibacterial modified disulfide siloxane was added to the nano-titanium dioxide dispersion, homogenized for 12 h, filtered, washed, and dried at 105 ° C for 6 h to obtain antibacterial modified TiO 2 Nano core-shell materials.

[0080] S2, 1 mL of deionized water, 1 mL of ammonia water and 2 mL of ethyl silicate were mixed in 5 mL of anhydrous ethanol under magnetic stirring for 20 min to obtain SiO 2 Precursor solution, add fluorinated polyurethane acrylate dropwise to SiO 2 In-situ polymerization was carried out in the precursor solution for 12 h, and antibacterial modified TiO 2 The nano core-shell material is uniformly dispersed in the mixed solution through ultrasonic treatment to obtain a coating.

[0081] Comparative Example 1

[0082] A corrosion-resistant coating on the surface of an aluminum alloy is obtained by coating, curing and drying the coating, wherein the coating comprises the following raw materials in parts by weight:

[0083] Polyurethane acrylate 50 parts;

[0084] 0.5 parts of antibacterial modified disulfide siloxane;

[0085] 2 parts of nano titanium dioxide;

[0086] 46.73 parts of ethyl silicate;

[0087] 22.5 parts of ammonia water;

[0088] 98.8 parts of anhydrous ethanol;

[0089] 10 parts of deionized water.

[0090] The steps for preparing the coating are as follows:

[0091] S1. 4 g of nano-titanium dioxide was uniformly dispersed in a mixture of 10 mL of deionized water and 10 mL of anhydrous ethanol by ultrasonic treatment. 300 μL of antibacterial modified disulfide siloxane was added to the nano-titanium dioxide dispersion, homogenized for 12 h, filtered, washed, and dried at 105 ° C for 6 h to obtain antibacterial modified TiO 2 Nano core-shell materials.

[0092] S2, 1 mL of deionized water, 1 mL of ammonia water and 2 mL of ethyl silicate were mixed in 5 mL of anhydrous ethanol under magnetic stirring for 20 min to obtain SiO 2 Precursor solution: 2 g polyurethane acrylate was added dropwise to SiO 2 In-situ polymerization in the precursor, reaction for 12 h, adding antibacterial modified TiO 2 The nano core-shell material is uniformly dispersed in the mixed solution through ultrasonic treatment to obtain a coating.

[0093] The difference between this comparative example and Example 1 is that no fluorinated polyurethane acrylate is added, but polyurethane acrylate that is not fluorinated is used.

[0094] Comparative Example 2

[0095] A corrosion-resistant coating on the surface of an aluminum alloy is obtained by coating, curing and drying the coating, wherein the coating comprises the following raw materials in parts by weight:

[0096] 50 parts of fluorinated polyurethane acrylate;

[0097] Contains 0.5 parts of disulfide bond polysiloxane;

[0098] 2 parts of nano titanium dioxide;

[0099] 46.73 parts of ethyl silicate;

[0100] 22.5 parts of ammonia water;

[0101] 98.8 parts of anhydrous ethanol;

[0102] 10 parts of deionized water.

[0103] The steps for preparing the coating are as follows:

[0104] S1. 4 g of nano-titanium dioxide was uniformly dispersed in a mixture of 10 mL of deionized water and 10 mL of anhydrous ethanol by ultrasonic treatment. 300 μL of disulfide-bonded polysiloxane was added to the nano-titanium dioxide dispersion, homogenized for 12 h, filtered, washed, and dried at 105 °C for 6 h to obtain modified TiO 2 Nano core-shell materials.

[0105] S2, 1 mL of deionized water, 1 mL of ammonia water and 2 mL of ethyl silicate were mixed in 5 mL of anhydrous ethanol under magnetic stirring for 20 min to obtain SiO 2 Precursor solution, add fluorinated polyurethane acrylate dropwise to SiO 2 In-situ polymerization was carried out in the precursor solution for 12 h, and modified TiO 2 The nano core-shell material is uniformly dispersed in the mixed solution through ultrasonic treatment to obtain a coating.

[0106] The difference between this comparative example and Example 1 is that no antibacterial modified disulfide siloxane is added as the preparation of modified TiO 2 The shell material of the nano core-shell material is not a disulfide bond-containing polysiloxane, an intermediate product of the preparation of antibacterial modified disulfide siloxane.

[0107] Comparative Example 3

[0108] A corrosion-resistant coating on the surface of an aluminum alloy is obtained by coating, curing and drying the coating, wherein the coating comprises the following raw materials in parts by weight:

[0109] 50 parts of fluorinated polyurethane acrylate;

[0110] 0.5 parts of perfluorooctyltriethoxysilane;

[0111] 0.03 parts of sodium pyrithione;

[0112] 2 parts of nano titanium dioxide;

[0113] 46.73 parts of ethyl silicate;

[0114] 22.5 parts of ammonia water;

[0115] 98.8 parts of anhydrous ethanol;

[0116] 10 parts of deionized water.

[0117] The steps for preparing the coating are as follows:

[0118] S1. 4 g of nano-titanium dioxide was uniformly dispersed in a mixture of 10 mL of deionized water and 10 mL of anhydrous ethanol by ultrasonic treatment. 300 μL of perfluorooctyl triethoxysilane and 0.06 g of sodium pyrithione were added to the nano-titanium dioxide dispersion, homogenized for 12 h, filtered, washed, and dried at 105 ° C for 6 h to obtain antibacterial modified TiO 2 Nano core-shell materials.

[0119] S2, 1 mL of deionized water, 1 mL of ammonia water and 2 mL of ethyl silicate were mixed in 5 mL of anhydrous ethanol under magnetic stirring for 20 min to obtain SiO 2 Precursor solution, add fluorinated polyurethane acrylate dropwise to SiO 2 In-situ polymerization was carried out in the precursor solution for 12 h, and antibacterial modified TiO 2 The nano core-shell material is uniformly dispersed in the mixed solution through ultrasonic treatment to obtain a coating.

[0120] The difference between this comparative example and Example 1 is that no antibacterial modified disulfide siloxane is added as the preparation method for antibacterial modified TiO 2 The shell material of the nano core-shell material is not made of perfluorooctyltriethoxysilane but of the antibacterial agent sodium pyrithione.

[0121] test:

[0122] 1. Electrochemical corrosion resistance test

[0123] The corrosion-resistant coating on the surface of the aluminum alloy was immersed in a simulated seawater solution for 14 days, and the electrochemical workstation (P3000A) was used to obtain EIS data to evaluate the electrochemical corrosion resistance of the corrosion-resistant coating on the surface of the aluminum alloy. Electrochemical impedance spectroscopy (EIS) is an important frequency domain research and testing method in corrosion science. It is one of the important methods for studying the electrochemical corrosion kinetics of metals, the corrosion mechanism of metals and coatings, and the corrosion resistance. The charge transfer resistance obtained in this experiment is recorded as R ct1 The greater the charge transfer resistance, the better the corrosion resistance.

[0124] 2. Microbiological Corrosion Resistance Test

[0125] First, SRB were incubated in a simulated seawater solution without SPT for 7 days, and the corrosion-resistant coating on the surface of the aluminum alloy was immersed in the simulated seawater solution for 14 days. The electrochemical workstation (P3000A) was used to obtain EIS data to evaluate the microbial corrosion resistance of the corrosion-resistant coating on the surface of the aluminum alloy. The charge transfer resistance obtained in this experiment was recorded as R ct2 The greater the charge transfer resistance, the better the corrosion resistance.

[0126] 3. Hydrophobicity test

[0127] The wettability of the corrosion-resistant coatings on the aluminum alloy surface was measured using a Dataphysics OCA 15EC Neurtek optical device by dropping ultrapure water (2 μL per drop) for contact angle measurements (n=10).

[0128] IV. Results Summary

[0129]

[0130] Table 1

[0131] V. Conclusion

[0132] 1. The charge transfer resistance of the electrochemical corrosion resistance test and the microbial corrosion resistance test of Examples 1-3 are much greater than those of Comparative Examples 2 and 3, but are not much different from Comparative Example 1, indicating that the presence of the antibacterial modified disulfide siloxane can significantly improve the electrochemical corrosion resistance test and microbial corrosion resistance of the corrosion-resistant coating on the surface of the aluminum alloy, and the fluorinated modified main resin can also play a certain role in corrosion resistance, but the degree of influence is not as great as that of the antibacterial modified disulfide siloxane.

[0133] 2. The contact angles of Examples 1-3 and Comparative Examples 2 and 3 are much larger than that of Comparative Example 1, reaching the standard of super-hydrophobicity, indicating that the fluorinated polyurethane acrylate plays a major role in super-hydrophobicity. Among them, the difference in contact angles between the coatings of Comparative Examples 2 and 3 and Examples 1-3 is small, indicating that the antibacterial modified disulfide siloxane can also play a certain hydrophobic role, but the degree of influence is far less than that of the fluorinated polyurethane acrylate.

[0134] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A corrosion-resistant coating on the surface of an aluminum alloy, characterized in that: The coating is obtained by coating, curing and drying. The coating includes the following raw materials in parts by weight: 40-60 parts of fluorinated polyurethane acrylate; Antibacterial modified disulfide siloxane 0.4-0.6 parts; Nano titanium dioxide 1.6-2.4 parts; Ethyl silicate 37.38-56.07 parts; 18-27 parts of ammonia water; Anhydrous ethanol 79-118.5 parts; 20-30 parts of deionized water.

2. The corrosion-resistant coating on the surface of an aluminum alloy according to claim 1, characterized in that: The preparation steps of the fluorinated polyurethane acrylate are as follows: 2 g of polyurethane acrylate and 0.2 g of triethyltriene were mixed in a homogeneous aqueous solution containing 3 mL of deionized water, 0.5 g of polytetrafluoroethylene and 20 μL of triethoxysilane were added dropwise to the aqueous solution, and then the mixture was magnetically stirred for 30 minutes to obtain fluorinated polyurethane acrylate.

3. The corrosion-resistant coating on the surface of an aluminum alloy according to claim 1, characterized in that: The preparation steps of the antibacterial modified disulfide siloxane are as follows: Step 1: Mix vinyl triethoxysilane and 3,3′-dithiodipropionic acid, raise the temperature to 90°C and stir magnetically under a nitrogen atmosphere, raise the temperature to 150°C and react for 20 minutes when the mixed system becomes clear and transparent, lower the temperature to 45°C and continue the reaction when distillate is produced, stop the reaction when no distillate is produced, lower the temperature to room temperature, and evacuate for 30 minutes to obtain a yellow viscous disulfide bond-containing polysiloxane; Step 2: prepare a PdCl2 / dimethyl sulfoxide mixed solvent, adjust the pH to 4-5 with PBS buffer, add pyrithione and the disulfide bond-containing polysiloxane prepared in step 1, and homogenize at 80°C for 2h under a nitrogen atmosphere to obtain an antibacterial modified disulfide siloxane.

4. The corrosion-resistant coating on the surface of an aluminum alloy according to claim 2, characterized in that: The mass ratio of vinyl triethoxysilane to 3,3′-dithiodipropionic acid in step 1 is 74.1:84.

11.

5. The corrosion-resistant coating on the surface of an aluminum alloy according to claim 2, characterized in that: In step 1, the concentration of PdCl2 in the PdCl2 / dimethyl sulfoxide mixed solvent is 0.025 mmol / mL, and the amount ratio of PdCl2 / dimethyl sulfoxide mixed solvent, pyrithione and disulfide bond-containing polysiloxane is 2 mL:0.5 mmol:1 mmol.

6. The corrosion-resistant coating on the surface of an aluminum alloy according to claim 1, characterized in that: The nano titanium dioxide is a rutile titanium dioxide nanorod with a particle size of 50nm; the purity of ethyl silicate is 99.9%; and the ammonia water is 27.3% ammonia water.

7. The corrosion-resistant coating on the surface of an aluminum alloy according to claim 1, characterized in that: The coating preparation steps are as follows: S1. 4 g of nano-titanium dioxide was uniformly dispersed in a mixture of 10 mL of deionized water and 10 mL of anhydrous ethanol by ultrasonic treatment, 250 μL of antibacterial modified disulfide siloxane was added to the nano-titanium dioxide dispersion, homogenized for 12 h, filtered, washed, and dried at 105 ° C for 6 h to obtain an antibacterial modified TiO2 nano core-shell material; S2. Deionized water, ammonia water and ethyl silicate are mixed in anhydrous ethanol under magnetic stirring for 20 minutes to obtain a SiO2 precursor solution, fluorinated polyurethane acrylate is added dropwise to the SiO2 precursor solution for in-situ polymerization, and the reaction is carried out for 12 hours. Antibacterial modified TiO2 nano core-shell material is added and uniformly dispersed in the above mixed solution by ultrasonic treatment to obtain a coating.

8. The corrosion-resistant coating on the surface of an aluminum alloy according to claim 7, characterized in that: In step S2, the dosage ratio of deionized water, ammonia water, ethyl silicate, anhydrous ethanol, fluorinated polyurethane acrylate and antibacterial modified TiO2 nano core-shell material is 10mL:10mL:20mL:50mL:20g:1g.

9. A method for preparing a corrosion-resistant coating on the surface of an aluminum alloy as claimed in any one of claims 1 to 8, characterized in that: The following steps are involved: (1) The surface of the aluminum alloy test piece with a thin plate structure was polished with 400, 600, 800, 1000, 1200, 2000 and 3000 mesh abrasive papers in sequence, and then ultrasonically cleaned in acetone for 5 minutes, rinsed with ethanol, and placed in a desiccator for standby use, thereby obtaining the aluminum alloy test piece after pretreatment; (2) Use a spray gun to spray the coating onto the pre-treated aluminum alloy specimen at a pressure of 0.4-0.6 MPa, and calcine at 180° C. for 20 minutes to obtain a corrosion-resistant coating on the aluminum alloy surface.

Citation Information

Cited By

  • Preparation method of plush-shaped anti-corrosion coating strongly attached to aluminum alloy surface

    CN120193316A