Low warping and scratch-resistant matte coating, low warping and scratch-resistant matte film and preparation method thereof

By applying low-warming deformation anti-scratch matte coating composed of acrylate prepolymers on the BOPP film, the mixed photocuring system and synergistic mechanism are used to solve the problem of insufficient warping deformation and adhesion of BOPP matte films. , achieves high adhesion and scratch resistance, meeting compound needs.

CN118909538BActive Publication Date: 2024-12-03GUANGDONG DECRO PACKAGE FILMS
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411374983.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-30
Publication Date
2024-12-03
Estimated Expiration
2044-09-30

AI Technical Summary

Technical Problem

Traditional BOPP matte films have problems such as warping and deformation and insufficient adhesion during filming, resulting in inconvenience and increased losses during use, making it difficult to meet the composite needs.

Method used

Low warping deformation anti-scratch matte coating, which consists of acrylate prepolymer, multifunctional hyperbranched active diluent, cationic photocuring monomer and modified matting agent, etc., and forms mutually through a hybrid photocuring system. Through the network structure, combining the synergistic effect of free radicals and cationic photoinitiators to reduce curing volume shrinkage and improve adhesion.

Benefits of technology

It effectively solves the problem of warping deformation and insufficient adhesion of BOPP scratch-resistant matte film, improves the scratch-resistant and wear resistance of the coating and meets the composite use needs of thinner BOPP scratch-resistant matte film, and ensures high Adhesion and low curing volume shrinkage.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The present invention relates to a low warping and scratch-resistant matte coating, a low warping and scratch-resistant matte film and a preparation method thereof, and belongs to the technical field of photocurable coatings. The low warping and scratch-resistant matte coating of the present invention comprises the following components by mass percentage: 23-40% acrylate prepolymer, 0.6-12% acrylate reactive monomer, 8-23% multifunctional hyperbranched reactive diluent, 15-23% cationic photocurable monomer, 3.5-7% modified matting agent, 0.7-2.3% free radical photoinitiator, 0.7-2.3% cationic photoinitiator, 0.5-1% organosilicon leveling agent, 10-20% solvent; wherein the multifunctional hyperbranched reactive diluent is formed by introducing acrylate functional groups through a polymer esterification reaction of polyhydroxy hyperbranched polyethylene and methacrylic acid. The low warping and deformation scratch-resistant matte coating of the present invention is coated on the surface of a BOPP film and light-cured to form a low warping and deformation scratch-resistant matte film. The film has a low volume shrinkage rate after curing, is not prone to warping and deformation, has good scratch resistance and wear resistance, and has an excellent matte effect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of photocurable coatings, and in particular to a low-warping and anti-scratch matte coating, a low-warping and anti-scratch matte film and a preparation method thereof. Background Art

[0002] BOPP matte film (gloss <5.0 at 60°) is widely accepted due to its soft and natural appearance, good visual effect and pleasant feel. However, the appearance, scratch resistance and wear resistance of traditional BOPP matte film can no longer meet the needs of customers.

[0003] BOPP matte film uses BOPP matting material to achieve a matte effect. BOPP matte material is a mixture of various polyolefins (mainly HDPE and PP). During the biaxial stretching process of film making, a rough surface morphology is produced due to the different crystallization rates and stretching responses of incompatible systems. The light irradiated on the rough surface is diffusely reflected to produce a matte effect, but the matte layer formed by BOPP matte material is not scratch-resistant. With the development of material technology and the change of aesthetics in the field of film packaging and printing, the use of scratch-resistant matte coatings to form a scratch-resistant matte layer on the surface of BOPP film, achieve a matte effect on BOPP film and give the surface scratch-resistant properties, has become an important development direction for BOPP matte film. Scratch-resistant matte coatings can be divided into two categories: water-based and solvent-based. At present, the scratch resistance of water-based scratch-resistant matte coatings is difficult to compare with solvent-based coatings, and they are not widely used in practice.

[0004] Traditional high-performance solvent-based scratch-resistant matte coatings usually have large volume shrinkage. This is because the light curing process of the coating is a transformation process from small molecules to long-chain or three-dimensional network macromolecules, and its molecular structure has undergone great changes. Before the anti-scratch matte coating is light-cured, the force between the components is van der Waals force, and the distance between molecules is van der Waals distance (0.3-0.5 nm); when the chemical reaction occurs and light curing occurs, the original intermolecular distance becomes a covalent bond distance (CC bond length average 0.154 nm), and the covalent bond distance is much smaller than the van der Waals force distance. The large change in the intermolecular distance leads to volume shrinkage during the curing process, which leads to product warping and deformation. With the implementation of environmental protection policies such as plastic reduction and lightweighting in the BOPP industry, BOPP film is developing in a thinner direction. The commonly used thickness is now below 12μm. The BOPP anti-scratch matte film produced by this has an increasing problem of warping and deformation. It is not easy to flatten when compounded with other materials. It is easy to produce wrinkles and other defects during composite use, causing great inconvenience and loss during use. Summary of the invention

[0005] Based on this, the purpose of the present invention is to provide a low warping and scratch-resistant matte coating, a low warping and scratch-resistant matte film and a preparation method thereof. The low warping and scratch-resistant matte coating of the present invention is coated on the surface of a BOPP film and light-cured to form a low warping and scratch-resistant matte film (also called a BOPP scratch-resistant matte film), which can solve the warping and deformation problem of the existing BOPP scratch-resistant matte film, improve the scratch resistance of the film surface, and give the film a matte appearance (glossiness <5.0 at 60°), especially meeting the composite use requirements of thinner BOPP scratch-resistant matte films.

[0006] In order to achieve the above object, the present invention adopts the following technical solutions:

[0007] The present invention first provides a low warpage and scratch-resistant matte coating, which comprises the following components by mass percentage: 23-40% of acrylate prepolymer, 0.6-12% of acrylate active monomer, 8-23% of multifunctional hyperbranched active diluent, 15-23% of cationic photocurable monomer, 3.5-7% of modified matting agent, 0.7-2.3% of free radical photoinitiator, 0.7-2.3% of cationic photoinitiator, 0.5-1% of organic silicon leveling agent, 1 0-20% solvent; wherein the multifunctional hyperbranched reactive diluent is formed by introducing acrylate functional groups through a high molecular esterification reaction of polyhydroxy hyperbranched polyethylene and methacrylic acid; the multifunctional hyperbranched reactive diluent has a number average molecular weight of 5000-20000 g / mol, a branching degree of (85-110) / 1000C, and a functionality of 5-7; the cationic light-curing monomer is an epoxy compound; and the modified matting agent contains an epoxy group.

[0008] The low warping and scratch-resistant matte coating provided by the present invention belongs to a hybrid photocuring system, which utilizes the synergistic mechanism of two curing methods. After ultraviolet light curing, a coating with an interpenetrating network structure (IPN) is obtained, which improves the scratch resistance of the coating and inhibits the volume shrinkage and warping deformation of the coating during curing.

[0009] The low warpage and scratch-resistant matte coating of the present invention is a hybrid photocurable scratch-resistant coating, which adopts the free radical photoinitiator and the cationic photoinitiator, provides two curing modes through the two photoinitiators, and utilizes the synergistic mechanism thereof, thereby overcoming the problems of slow curing speed and production difficulty of cationic polymerization, maintaining the respective advantages of free radical polymerization and cationic polymerization, and having fast curing speed, small volume shrinkage rate, and high mechanical strength. Among them, the free radical photoinitiator, under the irradiation of ultraviolet light, first generates a free radical active center to initiate free radical polymerization, and at the same time, the free radical fragments generated by the photolysis of the free radical photoinitiator can reduce the cationic photoinitiator, electron transfer occurs, indirect photolysis is achieved, a cationic active center is generated, and a cationic polymerization reaction is initiated. In addition to the electron transfer effect, the free radical photoinitiator can also directly photosensitize the cationic photoinitiator to a certain extent, thereby making full use of long-wave ultraviolet light and improving the curing speed of cationic polymerization.

[0010] The acrylate prepolymer has excellent flexibility and wear resistance, and can improve the mechanical properties of the coating formed by the low warpage anti-scratch matte coating. However, the viscosity of the acrylate prepolymer is large (generally above 2000 mPa•s), and the adhesion to the BOPP film is low. The present invention reduces the viscosity of the coating system by adding the acrylate reactive monomer and the multifunctional hyperbranched reactive diluent to the low warpage anti-scratch matte coating, and the acrylate prepolymer can polymerize with the acrylate reactive monomer and the multifunctional hyperbranched reactive diluent to form a cross-linking system, so that the coating formed by polymerization has good scratch resistance and high adhesion to the BOPP film, thereby improving the problems of poor production applicability and low adhesion of the coating caused by the high viscosity of the acrylate prepolymer.

[0011] Generally, the viscosity of the coating increases rapidly with the increase of the prepolymer content, and the mechanical properties are improved, but the high-viscosity coating is not suitable for thin film coating processing; the present invention adds the acrylate reactive monomer and the multifunctional hyperbranched reactive diluent to the low warpage anti-scratch matte coating to reduce the viscosity of the coating. The acrylate reactive monomer is a free radical reactive diluent (the viscosity is usually less than 50 mPa•s), which can significantly reduce the viscosity of the coating, and at the same time participates in the cross-linking reaction during the curing process to promote polymerization to form a cross-linking system. The amount of the acrylate reactive monomer added to the low warpage anti-scratch matte coating is 0.6-12wt%. Since the molecular weight of the acrylate reactive monomer is small, it is a small molecule reactive diluent. If the amount of the acrylate reactive monomer added is too large, the curing cross-linking density of the coating formed by the low warpage anti-scratch matte coating will be too large, the volume shrinkage of the coating will increase, resulting in problems such as brittle coating and decreased adhesion, and the product warpage is difficult to control.

[0012] The multifunctional hyperbranched reactive diluent is a functionalized hyperbranched polyethylene, which is formed by introducing acrylate functional groups through a high molecular esterification reaction between polyhydroxy hyperbranched polyethylene and methacrylic acid. The multifunctional hyperbranched reactive diluent, as a polyethylene-based copolymer, can effectively wet the surface of the BOPP film, and the multifunctional hyperbranched reactive diluent is in a non-crystalline state. After being attached to the surface of the BOPP film, it can diffuse into the inside of the BOPP film, entangle with the molecular chain segments on the surface of the BOPP film, and enhance the intermolecular force. The mutual entanglement between the molecular chain segments enhances the adhesion between the coating formed by the low warpage deformation anti-scratch matte coating and the BOPP film. The acrylate functional groups at the ends of the molecular chains of the multifunctional hyperbranched reactive diluent can participate in the free radical photocuring reaction, and are cross-linked to the coating through chemical bonds, which can effectively overcome the problems of excessive crosslinking density, large volume shrinkage, brittle coating and insufficient adhesion after free radical photocuring, and form an interpenetrating network structure (IPN) with cationic polymerization to obtain a coating with extremely low warpage deformation and high scratch resistance. The content of the multifunctional hyperbranched reactive diluent in the low warpage anti-scratch matte coating is 8-23wt%. If the content of the multifunctional hyperbranched reactive diluent is too low, it cannot reduce the viscosity of the coating and prevent the coating from becoming brittle, and cannot effectively improve the problem of low adhesion of the coating on the surface of the BOPP film; if the content of the multifunctional hyperbranched reactive diluent is too low, the cost increases, and at the same time the hardness of the coating decreases, affecting the scratch resistance of the coating.

[0013] The multifunctional hyperbranched reactive diluent described in the present invention is neither a multifunctional small molecule reactive diluent nor a linear high molecular prepolymer. The linear polyethylene molecular chain structure has high regularity and is very easy to crystallize, but as the degree of branching increases, the regularity of the polyethylene molecular chain structure is destroyed, so that the crystallinity of the polyethylene decreases, and the polyethylene molecular chain segments begin to be easy to thermally move. The present invention utilizes the above characteristics to limit the branching degree of the multifunctional hyperbranched reactive diluent to (85-110) / 1000C. The branching degree of the multifunctional hyperbranched reactive diluent forms a spherical topological structure at (85-110) / 1000C, is completely non-crystalline at room temperature, has good flow permeability, and has strong adhesion to BOPP film. The spherical topological structure of the multifunctional hyperbranched active diluent is dense in structure, small in fluid mechanics radius, no intrachain entanglement, small intermolecular friction compared with the linear macromolecules of random coils, thus realizing active dilution in the coating system and reducing viscosity; it is not easy to be entangled with the IPN system during the photocuring process, thus playing the role of active dilution and lubrication; the multifunctional hyperbranched active diluent is evenly distributed in the coating, the photocuring cross-linking reaction is complete, and the problem of residual unreacted free radicals is improved. The present invention limits the number average molecular weight of the multifunctional hyperbranched reactive diluent to between 5000 and 20000 g / mol. When the molecular weight of the multifunctional hyperbranched reactive diluent is too low, the topological structure of the polyethylene molecular segment in its structure tends to be linear, and it is easy to entangle with itself and the acrylate prepolymer in the coating system, and it does not play the role of a diluent; when the molecular weight of the multifunctional hyperbranched reactive diluent is too high, the multifunctional hyperbranched reactive diluent is difficult to dissolve in the coating system, and phase separation and stratification are easy to occur. The functionality of the multifunctional hyperbranched reactive diluent is 5-7, which can ensure that the crosslinking density is moderate. If the functionality is too large, it is easy to cause the coating crosslinking density to be too large, the volume shrinkage is large, and the coating becomes brittle and the adhesion is insufficient.

[0014] When the cationic photocurable monomer, i.e., the epoxy compound, undergoes cationic ring-opening polymerization initiated by light, two CO covalent bonds on the alicyclic ring are broken and intermolecular covalent bonds are generated simultaneously, and the distance between molecules does not change significantly. Therefore, the epoxy compound has a very small volume shrinkage during the polymerization reaction, and effectively controls the volume shrinkage of free radical polymerization in the coating of the IPN system, thereby inhibiting the warping deformation of the product. The cationic photocurable monomer, i.e., the epoxy compound, is added in an amount of 15-23wt% in the low warping and scratch-resistant matte coating, which can ensure that the low warping and scratch-resistant matte coating has a low viscosity and good production applicability, while satisfying the requirement of small volume shrinkage during coating curing, thereby overcoming the problem of product warping deformation. If the cationic photocurable monomer is added in an excessive amount in the low warping and scratch-resistant matte coating, due to the high viscosity of the cationic photocurable monomer (generally above 200mPa•s), it is easy to cause the viscosity of the low warping and scratch-resistant matte coating to be too high, and the high viscosity coating is not suitable for the coating process of BOPP film.

[0015] The modified matting agent contains epoxy groups, which have good compatibility with the coating system and will not cause a sharp increase in the viscosity of the coating system. The epoxy groups on the modified matting agent are cross-linked to the interpenetrating network (IPN) structure of the coating by chemical bonds during photoinduced cationic ring-opening polymerization. After curing, the coating does not fall off and has high hardness, which greatly improves the scratch resistance and wear resistance of the coating and gives the coating an excellent matte effect.

[0016] Furthermore, the acrylate prepolymer is an aliphatic polyurethane acrylate, and the functionality of the aliphatic polyurethane acrylate is 2-4 and the molecular weight is 1000 g / mol. The present invention uses an aliphatic polyurethane acrylate with a functionality of 2-4, so that the coating formed by the low warpage deformation scratch-resistant matte coating has good scratch resistance and good coating flexibility. If the functionality of the aliphatic polyurethane acrylate is too high, although the coating formed by the polymerization thereof has a large cross-linking density, a large hardness, and good scratch resistance, the excessive cross-linking density will lead to the problem of brittle coating and reduced flexibility.

[0017] Furthermore, the acrylate reactive monomer is a difunctional or trifunctional acrylate compound. Preferably, the acrylate reactive monomer is one or more of EGDA (ethylene glycol diacrylate, viscosity: 8 mPa•s), NPGDA (neopentyl glycol diacrylate, viscosity: 10 mPa•s), TPGDA (tripropylene glycol diacrylate, viscosity: 13 mPa•s), and ETPTA (ethoxylated trihydroxymethylpropane triacrylate, viscosity: 25 mPa•s). The above-mentioned difunctional or trifunctional acrylate compound is a free radical type reactive diluent with a small molecular weight, which can significantly reduce the viscosity of the coating, prevent the curing crosslinking density of the coating formed by the low warpage deformation anti-scratch matte coating from being too large, prevent the volume shrinkage of the coating from increasing, and improve the problems of brittleness and decreased adhesion of the coating.

[0018] Furthermore, the multifunctional hyperbranched active diluent is prepared by the following steps: catalyzing the copolymerization reaction of ethylene and acrylate monomers with silane-protected hydroxyl groups under the action of a late transition metal palladium-diimine catalyst, and the product is precipitated with ethanol to obtain a colorless transparent oily substance; then the colorless transparent oily substance is treated with a tetra-n-butylammonium fluoride solution to remove the protection of the hydroxyl group to obtain a polyhydroxy hyperbranched polyethylene containing multiple hydroxyl groups, and the polyhydroxy hyperbranched polyethylene and methacrylic acid are introduced into the acrylate functional group through a polymer esterification reaction to form the multifunctional hyperbranched active diluent. The multifunctional (functionality 5-7) hyperbranched active diluent obtained by the present invention using the late transition metal palladium-diimine catalytic polymerization has a spherical topological structure, is completely non-crystalline at room temperature, has good flow permeability, and has strong adhesion to BOPP film.

[0019] Furthermore, the cationic photocurable monomer is one or two of EEC (3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexylcarboxylate) and BEA (di(3,4-epoxycyclohexylmethyl)adipate). Both EEC (3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexylcarboxylate) and BEA (di(3,4-epoxycyclohexylmethyl)adipate) are epoxy compounds, which can simultaneously break two CO covalent bonds on the alicyclic ring and generate intermolecular covalent bonds during photoinduced cationic ring-opening polymerization, and the intermolecular distance changes little, so the volume shrinkage is small during the polymerization process, and plays a good role in inhibiting the volume shrinkage and warping deformation of the coating during curing in the hybrid photocurable coating system of the present invention.

[0020] Further, the modified matting agent is a silane coupling agent modified silica particles; in the silane coupling agent modified silica particles, the silane coupling agent is a silane coupling agent containing an epoxy group, and the amount of the silane coupling agent is 0.5-3wt% of the silica particles; the particle size of the modified matting agent is 1-2μm. Preferably, the modified matting agent is a silane coupling agent KH-560 modified silica particles, as a specific modification method: add the silane coupling agent KH-560 to ethanol, adjust the pH to 7-9, add silica particles, ultrasonicate for 30 minutes, stir for 10 minutes (speed <200 r / min), heat to 120 ° C after fully wetting, high-speed shear dispersion for 30 minutes (speed>5000 r / min), filter after cooling, rinse with ethanol, dry under vacuum for 4 hours, grind and disperse with a ball mill to obtain silane coupling agent KH-560 modified silica particles. The present invention adopts silane coupling agent modified silica particles as modified matting agent, which has good compatibility with the coating system and will not cause a sharp increase in the viscosity of the coating system. The silane coupling agent KH-560 contains an epoxy group at the end. The silane coupling agent KH-560 modified silica particles are used as modified matting agent. During photoinduced cationic ring-opening polymerization, the silane coupling agent KH-560 is cross-linked to the interpenetrating network (IPN) structure of the coating by chemical bonds. After curing, the coating does not fall off and has high hardness, which greatly improves the scratch resistance and wear resistance of the coating.

[0021] Further, the free radical photoinitiator is one or more of benzoin, benzoin ether, acetophenone, and acetophenone ketal compounds. Preferably, the free radical photoinitiator is one or more of photoinitiator 184, photoinitiator 1173, photoinitiator TPO, and photoinitiator 907. These free radical photoinitiators can effectively generate free radicals during the photocuring process to promote the rapid curing of the coating.

[0022] Further, the cationic photoinitiator is one or more of diaryliodonium salts, triarylsulfonium salts, and alkylsulfonium salt compounds. Preferably, the cationic photoinitiator is one or more of photoinitiator PAG208, photoinitiator PAG202, photoinitiator UVI6976, and photoinitiator UVI6974. These cationic photoinitiators can effectively generate cations under the irradiation of ultraviolet light, thereby initiating and accelerating cationic polymerization reactions.

[0023] Furthermore, the solvent is one or more of butanone, ethyl acetate, and butyl acetate. The above solvents can evenly disperse the components of the coating, adjust the viscosity and coating properties of the coating, and the above solvents have a low boiling point, which helps to dry the coating to remove the solvent after coating, and form a coating through photocuring.

[0024] The present invention also provides a low warping and scratch-resistant matte film (also called BOPP scratch-resistant matte film), comprising a coating and a BOPP film layer; the coating is formed by coating any of the above-mentioned low warping and scratch-resistant matte coatings on the surface of the BOPP film layer; the BOPP film layer is a BOPP film.

[0025] The low warping and deformation scratch-resistant film of the present invention solves the problems of warping and deformation of the existing BOPP scratch-resistant matte film and insufficient adhesion of the coating on the surface of the BOPP film. The low warping and deformation scratch-resistant matte film of the present invention improves the scratch resistance and wear resistance of the coating, has high adhesion between the coating and the BOPP film, is not prone to warping and deformation, and meets the high-end composite requirements of the BOPP scratch-resistant matte film.

[0026] Furthermore, the dry weight of the coating is 1-4 g / m 2 The thickness of the BOPP film layer is 8-12 μm. The dry weight of the coating on the thinner (8-12 μm) BOPP film surface is 1-4 g / m 2 The coating produces a low warping and scratch-resistant matte film (BOPP scratch-resistant matte film), which is not prone to warping and deformation, and is easy to flatten when compounded with other materials, improving wrinkles and other defects during composite use, especially meeting the composite use needs of thinner BOPP scratch-resistant matte films.

[0027] The present invention also provides a method for preparing any of the above-mentioned low warping and scratch-resistant matt films, comprising the following steps:

[0028] S1: preparing any of the above-mentioned low warpage and scratch-resistant matte coatings;

[0029] S2: coating the low warpage and anti-scratch matte coating on the surface of the BOPP film, drying the solvent, and curing with ultraviolet light to obtain the low warpage and anti-scratch matte film.

[0030] Furthermore, the solvent is dried by heating in an oven at 70-80°C for 40-60s, and then cured by ultraviolet light for 40-60s to form a matte anti-scratch layer. If the drying temperature is too low, the drying efficiency will be affected, and if the drying temperature is too high, the quality of the low warpage anti-scratch matte film will be adversely affected, such as discoloration and oxidation of the product.

[0031] Compared with existing technology:

[0032] The low warping and anti-scratch coating of the present invention has good fluidity, meets the requirements of traditional mature industrial coating processes such as roller coating, spray coating, and scraper coating, is simple and easy to use, and has strong practicality and commercial prospects. The low warping and anti-scratch matte coating of the present invention is coated on the surface of the BOPP film and light-cured to form a low warping and anti-scratch matte film (also called BOPP anti-scratch matte film). The film has a low volume shrinkage rate after curing, is not easy to warp and deform, has good scratch resistance and wear resistance, and has an excellent matte effect. DETAILED DESCRIPTION

[0033] In order to facilitate the understanding of the present invention, the present invention will be described more fully below. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein.

[0034] The invention provides a low-warping and anti-scratch matte coating, which comprises the following components by mass percentage: 23-40% of acrylate prepolymer, 0.6-12% of acrylate active monomer, 8-23% of multifunctional hyperbranched active diluent, 15-23% of cationic photocuring monomer, 3.5-7% of modified matting agent, 0.7-2.3% of free radical photoinitiator, 0.7-2.3% of cationic photoinitiator, 0.5-1% of organic silicon leveling agent, and 10-20% of solvent; wherein the multifunctional hyperbranched active diluent is formed by introducing acrylate functional groups through high molecular esterification reaction of polyhydroxy hyperbranched polyethylene and methacrylic acid; the multifunctional hyperbranched active diluent has a number average molecular weight of 5000-20000, a branching degree of (85-110) / 1000C, and a functionality of 5-7; and the cationic photocuring monomer is an epoxy compound.

[0035] The preparation method of the multifunctional hyperbranched active diluent comprises the following steps: catalyzing the copolymerization reaction of ethylene and acrylate monomers with silane-protected hydroxyl groups under the action of a late transition metal palladium-diimine catalyst, and obtaining a colorless transparent oily substance after the product is precipitated by ethanol; then treating the colorless transparent oily substance with a tetra-n-butylammonium fluoride solution to remove the protection of the hydroxyl group, thereby obtaining a multi-hydroxy hyperbranched polyethylene containing multiple hydroxyl groups; and introducing an acrylate functional group into the multi-hydroxy hyperbranched polyethylene and methacrylic acid through a high molecular esterification reaction, thereby forming the multifunctional hyperbranched active diluent.

[0036] Among them, taking a multifunctional hyperbranched active diluent with a number average molecular weight of 20000g / mol, a branching degree of 100 / 1000C, and a functionality of 7 as an example, the specific operation process is as follows: a low-pressure glass reactor is connected to a circulating vacuum pump, and high-temperature drying is performed under infrared light for more than 3 hours, and then cold pumping is performed for 1 hour to keep the glass reactor absolutely dry. 100 mmol of late transition metal palladium-diimine catalyst is dissolved in anhydrous dichloromethane. Under nitrogen protection, the dichloromethane solution containing the catalyst and 0.02 mol of trimethylsilane-protected hydroxyethyl acrylate (HEA-TMS) monomer solution are added to a dry and sealed glass reactor, and ethylene is introduced to control the set pressure to 0.1-5 atm, and the temperature is set to 0-5°C. After reacting in a constant temperature water bath for 24 hours, a small amount of ethanol is added to terminate the reaction to obtain a mixture of copolymers containing ethylene and HEA-TMS. After dissolving the above mixture with an appropriate amount of dichloromethane, pour it into cold anhydrous ethanol for precipitation, and let it stand until the precipitation is complete to remove the catalyst and comonomer to obtain a colorless transparent oil. The above colorless transparent oil is dissolved in 100 ml of tetrahydrofuran, the dissolution time is 2-3 hours, and tetrabutylammonium fluoride tetrahydrofuran solution is added. After 1 hour, concentrated hydrochloric acid is added. After 0.5 hours, the reaction is stopped, the product is separated, and an excess of methanol is added to precipitate the polymer, which is washed with methanol several times and dried in a vacuum oven to obtain a multi-hydroxy hyperbranched polyethylene; then the prepared multi-hydroxy hyperbranched polyethylene is reacted with methacrylic acid through a polymer esterification reaction to introduce acrylate functional groups to obtain a multi-functional hyperbranched active diluent with a number average molecular weight of 20000g / mol, a branching degree of 100 / 1000C, and a functionality of 7. The preparation of multifunctional hyperbranched reactive diluents with other number average molecular weights, branching degrees, and functionalities can be controlled by regulating the polymerization time, ethylene pressure, and polymerization temperature, which can be routinely adjusted by those skilled in the art according to the above preparation method and will not be described in detail here.

[0037] The modified matting agents used in the following examples or comparative examples are all silica particles modified by silane coupling agent KH-560, and the amount of silane coupling agent KH-560 is 2wt% of the silica particles; the average particle size of the modified matting agent is 2μm.

[0038] The specific modification method of the silica particles modified by the silane coupling agent KH-560 is as follows: the silane coupling agent KH-560 is added to ethanol, the pH is adjusted to 7-9, the silica particles are added, ultrasonicated for 30 minutes, stirred for 10 minutes (speed <200 r / min), the temperature is raised to 120°C after sufficient wetting, high-speed shear dispersion is performed for 30 minutes (speed >5000 r / min), filtered after cooling, rinsed with ethanol, dried under vacuum for 4 hours, and ground and dispersed with a ball mill to obtain silica particles modified by the silane coupling agent KH-560.

[0039] Example 1

[0040] The present embodiment provides a low warpage and scratch-resistant matte coating, which includes the following components by mass percentage: 40% acrylate prepolymer (aliphatic polyurethane acrylate, molecular weight 1000 g / mol), 12% acrylate active monomer (EGDA), 8% multifunctional hyperbranched active diluent (number average molecular weight Mn: 20000 g / mol, branching degree: 100 / 1000C, functionality: 7), 23% cationic photocurable monomer (EEC), 4.3% modified matting agent, 0.7% free radical photoinitiator (photoinitiator 184), 1.5% cationic photoinitiator (photoinitiator UVI6974), 0.5% silicone leveling agent, and 10% solvent (butyl acetate).

[0041] This embodiment also provides a low warping and scratch-resistant matte film, comprising a coating and a BOPP film layer, wherein the coating is formed by coating the above-mentioned low warping and scratch-resistant matte coating on the surface of the BOPP film layer; and the BOPP film layer is a BOPP film.

[0042] This embodiment also provides a method for preparing a low-warping and anti-scratch matte film, comprising the following steps:

[0043] S1: According to the mass percentage components of the low warpage and scratch-resistant matte coating of this embodiment, the raw materials of each component are added into a constant temperature sealed high-speed stirring tank and stirred to obtain the low warpage and scratch-resistant matte coating; wherein the stirring speed is 1500 rpm, the temperature is controlled at 30° C., and the stirring time is 4 hours;

[0044] S2: The low warpage and anti-scratch matte coating is coated on the surface of a 12 μm thick BOPP film using a coating machine with a micro-concave roller coating method; the solvent is dried by heating in an oven at 70° C. for 50 seconds, and cured by ultraviolet light irradiation for 40 seconds to form a BOPP anti-scratch matte film, i.e., the low warpage and anti-scratch matte film.

[0045] In the low warpage and scratch-resistant matt film of this embodiment, the dry weight of the coating is 1.5 g / m 2 .

[0046] Example 2

[0047] The present embodiment provides a low warpage and scratch-resistant matte coating, which includes the following components by mass percentage: 30% acrylate prepolymer (aliphatic polyurethane acrylate, molecular weight 1000 g / mol), 0.6% acrylate reactive monomer (ETPTA), 23% multifunctional hyperbranched reactive diluent (number average molecular weight Mn: 5500 g / mol, branching degree: 86 / 1000C, functionality: 5), 20% cationic photocurable monomer (BEA), 4% modified matting agent, 1.2% free radical photoinitiator (photoinitiator TPO), 0.7% cationic photoinitiator (photoinitiator UVI6976), 0.5% silicone leveling agent, and 20% solvent (ethyl acetate).

[0048] This embodiment also provides a low warping and scratch-resistant matte film, comprising a coating and a BOPP film layer, wherein the coating is formed by coating the above-mentioned low warping and scratch-resistant matte coating on the surface of the BOPP film layer; and the BOPP film layer is a BOPP film.

[0049] This embodiment also provides a method for preparing a low-warping and anti-scratch matte film, comprising the following steps:

[0050] S1: According to the mass percentage components of the low warpage and scratch-resistant matte coating of this embodiment, the raw materials of each component are added into a constant temperature sealed high-speed stirring tank and stirred to obtain the low warpage and scratch-resistant matte coating; wherein the stirring speed is 1500 rpm, the temperature is controlled at 30° C., and the stirring time is 3 hours;

[0051] S2: The low warpage and scratch-resistant matte coating is coated on the surface of a 10 μm thick BOPP film by using a coating machine and a micro-concave roller coating method; the solvent is dried by heating in an oven at 80° C. for 60 seconds, and cured by ultraviolet light for 60 seconds to form a BOPP scratch-resistant matte film, i.e., the low warpage and scratch-resistant matte film.

[0052] In the low warpage and scratch-resistant matt film of this embodiment, the dry weight of the coating is 3.5 g / m 2 .

[0053] Example 3

[0054] The present embodiment provides a low warpage and scratch-resistant matte coating, which includes the following components by mass percentage: 23% acrylate prepolymer (aliphatic polyurethane acrylate, molecular weight 1000 g / mol), 10% acrylate reactive monomer (ETPTA), 15% multifunctional hyperbranched reactive diluent (number average molecular weight Mn: 10000 g / mol, branching degree: 95 / 1000C, functionality: 6), 22% cationic photocurable monomer (BEA), 7% modified matting agent, 2.3% free radical photoinitiator (photoinitiator TPO), 2.3% cationic photoinitiator (photoinitiator UVI6976), 1% silicone leveling agent, and 17.4% solvent (butanone).

[0055] This embodiment also provides a low warping and scratch-resistant matte film, comprising a coating and a BOPP film layer, wherein the coating is formed by coating the above-mentioned low warping and scratch-resistant matte coating on the surface of the BOPP film layer; and the BOPP film layer is a BOPP film.

[0056] This embodiment also provides a method for preparing a low-warping and anti-scratch matte film, comprising the following steps:

[0057] S1: According to the mass percentage components of the low warpage and scratch-resistant matte coating of this embodiment, the raw materials of each component are added into a constant temperature sealed high-speed stirring tank and stirred to obtain the low warpage and scratch-resistant matte coating; wherein the stirring speed is 1500 rpm, the temperature is controlled at 30° C., and the stirring time is 3 hours;

[0058] S2: The low warpage and anti-scratch matte coating is coated on the surface of a 10 μm thick BOPP film by using a coating machine and a micro-concave roller coating method; the solvent is dried by heating in an oven at 80° C. for 50 seconds, and cured by ultraviolet light for 50 seconds to form a BOPP anti-scratch matte film, i.e., the low warpage and anti-scratch matte film.

[0059] In the low warpage and scratch-resistant matt film of this embodiment, the dry weight of the coating is 2.5 g / m 2 .

[0060] Comparative Example 1

[0061] The present comparative example provides a photocurable matte coating, which comprises the following components by mass percentage: 40% acrylate prepolymer (aliphatic polyurethane acrylate, molecular weight of 1000 g / mol), 35% acrylate reactive monomer (EGDA), 8% multifunctional hyperbranched reactive diluent (number average molecular weight Mn: 20000 g / mol, degree of branching: 100 / 1000C, functionality: 7), 4.3% modified matting agent, 2.2% free radical photoinitiator (photoinitiator 184), 0.5% organosilicon leveling agent, and 10% solvent (butyl acetate).

[0062] This comparative example also provides a photocurable matte film, comprising a coating and a BOPP film layer, wherein the coating is formed by coating the above-mentioned photocurable matte coating on the surface of the BOPP film layer; and the BOPP film layer is a BOPP film.

[0063] This comparative example also provides a method for preparing a photocurable matte film, comprising the following steps:

[0064] S1: According to the mass percentage components of the light-curing matte coating of this comparative example, the raw materials of each component are added into a constant temperature sealed high-speed stirring tank and stirred to obtain the light-curing matte coating; wherein the stirring speed is 1500 rpm, the temperature is controlled at 30° C., and the stirring time is 4 hours;

[0065] S2: The above-mentioned light-curable matte coating is coated on the surface of a 12 μm thick BOPP film by using a coating machine with a micro-concave roller coating method; the solvent is dried by heating in an oven at 70° C. for 50 seconds, and cured by ultraviolet light irradiation for 40 seconds to form the above-mentioned light-curable matte film.

[0066] In the photocurable matte film of this comparative example, the dry weight of the coating is 1.5 g / m 2 .

[0067] Comparative Example 2

[0068] The present comparative example provides a photocurable matte coating, which comprises the following components by mass percentage: 40% acrylate prepolymer (aliphatic polyurethane acrylate, molecular weight 1000 g / mol), 20% acrylate active monomer (EGDA), 23% cationic photocurable monomer (EEC), 4.3% modified matting agent, 0.7% free radical photoinitiator (photoinitiator 184), 1.5% free radical photoinitiator (photoinitiator UVI6974), 0.5% silicone leveling agent, and 10% solvent (butyl acetate).

[0069] This comparative example also provides a photocurable matte film, comprising a coating and a BOPP film layer, wherein the coating is formed by coating the above-mentioned photocurable matte coating on the surface of the BOPP film layer; and the BOPP film layer is a BOPP film.

[0070] This comparative example also provides a method for preparing a photocurable matte film, comprising the following steps:

[0071] S1: According to the mass percentage components of the light-curing matte coating of this comparative example, the raw materials of each component are added into a constant temperature sealed high-speed stirring tank and stirred to obtain the light-curing matte coating; wherein the stirring speed is 1500 rpm, the temperature is controlled at 30° C., and the stirring time is 4 hours;

[0072] S2: The above-mentioned light-curable matte coating is coated on the surface of a 12 μm thick BOPP film by using a coating machine with a micro-concave roller coating method; the solvent is dried by heating in an oven at 70° C. for 50 seconds, and cured by ultraviolet light irradiation for 40 seconds to form the above-mentioned light-curable matte film.

[0073] In the photocurable matte film of this comparative example, the dry weight of the coating is 1.5 g / m 2 .

[0074] Performance Testing

[0075] The following performance tests were performed on the matte coatings and matte films of Examples 1-3 and Comparative Examples 1-2, respectively. Please refer to Tables 1 and 2 for the results.

[0076] Pencil hardness: Test the pencil hardness of the coating according to the standard of JIS K5400-1990 "Determination of adhesion properties of powder coating films".

[0077] Gloss: According to GB / T 9754-2007, measured using a 60° gloss meter.

[0078] Adhesion of coating: According to the standard of GB1720-1979 "Determination of adhesion of paint films", the adhesion of coating is tested, where 100 / 100 means no film peeling, and 90 / 100 means 10% peeling.

[0079] Scratch resistance / wear resistance test: According to HG / T 4303-2012 "Test method for wear resistance of surface hardened polyester film", the wear resistance of the coating was tested using 0000# steel wool, 1000gf / cm 2 The wear resistance of the film can be judged by testing the limit of the number of times the diaphragm surface can be worn without scratches.

[0080] Volume shrinkage test: Test in accordance with the relevant provisions of international standard ISO 3521.

[0081] Table 1 Matte coating test of Examples 1-3 and Comparative Examples 1-2

[0082]

[0083] Table 2 Matt film test of Examples 1-3 and Comparative Examples 1-2

[0084]

[0085] It is well known to those skilled in the art that the existing commonly used low warping and scratch-resistant matte coatings usually have a volume shrinkage rate greater than 5%. The BOPP scratch-resistant matte film prepared by coating it on the surface of a thinner BOPP film has a large warping and deformation problem.

[0086] It can be seen from the test data in Table 1 and Table 2 that the low warpage and scratch-resistant matte coatings of Examples 1-3 of the present invention have good fluidity, a viscosity of ≤450 mPa•s (30°C), and a low curing volume shrinkage of ≤3%. The low warpage and scratch-resistant matte films (BOPP scratch-resistant matte films) produced in Examples 1-3 of the present invention effectively improve the warpage problem, and at the same time, the coating has qualified adhesion to the BOPP film, low appearance gloss, and excellent scratch / wear resistance.

[0087] In the photocurable matte coating of Comparative Example 1, no cationic photocurable monomer and cationic photoinitiator are added. It is a pure free radical photocurable scratch-resistant matte coating. The produced photocurable matte film has severe warping and deformation. At the same time, due to the lack of interpenetrating network structure (IPN) generated by simultaneous polymerization of cationic species, the scratch resistance of the photocurable matte film of Comparative Example 1 is reduced.

[0088] In the photocurable matte coating of Comparative Example 2, no multifunctional hyperbranched reactive diluent is added. The coating formed by the photocurable matte coating of Comparative Example 2 lacks components that promote adhesion to the BOPP film. When the coating is partially peeled off using a tape test, the adhesion to the BOPP film is unqualified. At the same time, since the photocurable coating of Comparative Example 2 uses a large amount of small molecule reactive diluent (i.e., acrylate reactive monomer) in order to maintain the low viscosity state of the coating, the volume shrinkage after curing is difficult to be suppressed by the IPN system, the solid volume shrinkage rate is slightly higher, and the degree of film warping deformation is greater than that of Examples 1-3.

[0089] Compared with the prior art, the low warpage anti-scratch matte coating of the present invention uses a general coating process, is coated on the surface of the BOPP film once, and forms a low warpage anti-scratch matte film after light curing. It can solve the serious warpage problem of the existing BOPP anti-scratch matte film and the problem of insufficient adhesion of the coating on the surface of the BOPP film, improve the scratch resistance / wear resistance of the coating, and at the same time give the film an excellent matte effect, meeting the high-end composite requirements of BOPP anti-scratch matte film. The low warpage anti-scratch matte coating has good fluidity, viscosity ≤ 450 mPa•s, and has a low curing volume shrinkage rate, the volume shrinkage rate after curing is ≤3%, and can be applied to thinner BOPP films for the preparation of low warpage BOPP anti-scratch matte films.

[0090] The above-mentioned embodiments only express several implementation methods of the present invention, and the description is relatively specific and detailed, but it cannot be understood as limiting the scope of the invention patent. It should be pointed out that for ordinary technicians in this field, several modifications and improvements can be made without departing from the concept of the present invention, and the present invention is also intended to include these modifications and modifications.

Claims

1. A low warping and scratch-resistant matte coating, characterized in that: The composition comprises the following components by mass percentage: 23-40% acrylate prepolymer, 0.6-12% acrylate active monomer, 8-23% multifunctional hyperbranched active diluent, 15-23% cationic photocurable monomer, 3.5-7% modified matting agent, 0.7-2.3% free radical photoinitiator, 0.7-2.3% cationic photoinitiator, 0.5-1% organosilicon leveling agent, and 10-20% solvent; The multifunctional hyperbranched reactive diluent is formed by introducing acrylate functional groups through a polymer esterification reaction between polyhydroxy hyperbranched polyethylene and methacrylic acid; the number average molecular weight of the multifunctional hyperbranched reactive diluent is 5000-20000 g / mol, the degree of branching is (85-110) / 1000C, and the functionality is 5-7; the cationic light-curing monomer is an epoxy compound; and the modified matting agent contains epoxy groups.

2. The low warpage and scratch-resistant matte coating according to claim 1, characterized in that: The acrylate prepolymer is aliphatic polyurethane acrylate, the functionality of the aliphatic polyurethane acrylate is 2-4, and the molecular weight of the aliphatic polyurethane acrylate is 1000 g / mol.

3. The low warping and scratch-resistant matte coating according to claim 1, characterized in that: The acrylate reactive monomer is one or more of ethylene glycol diacrylate, neopentyl glycol diacrylate, tripropylene glycol diacrylate, and ethoxylated trihydroxymethylpropane triacrylate.

4. The low warping and scratch-resistant matte coating according to claim 1, characterized in that: The multifunctional hyperbranched active diluent is prepared by the following steps: catalyzing the copolymerization reaction of ethylene and acrylate monomers with silane-protected hydroxyl groups under the action of a late transition metal palladium-diimine catalyst, and obtaining a colorless transparent oily substance after the product is precipitated by ethanol; then treating the colorless transparent oily substance with a tetra-n-butylammonium fluoride solution to remove the protection of the hydroxyl group, thereby obtaining a polyhydroxy hyperbranched polyethylene containing multiple hydroxyl groups; and introducing an acrylate functional group into the polyhydroxy hyperbranched polyethylene and methacrylic acid through a high molecular esterification reaction, thereby forming the multifunctional hyperbranched active diluent.

5. The low warping and scratch-resistant matte coating according to claim 1, characterized in that: The cationic photocurable monomer is one or two of 3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexylcarboxylate and di(3,4-epoxycyclohexylmethyl)adipate.

6. The low warping and scratch-resistant matte coating according to claim 1, characterized in that: The modified matting agent is a silane coupling agent modified silica particle; in the silane coupling agent modified silica particle, the silane coupling agent is a silane coupling agent containing an epoxy group; the amount of the silane coupling agent is 0.5-3wt% of the silica particle; the particle size of the modified matting agent is 1-2μm.

7. The low warpage and scratch-resistant matte coating according to claim 1, characterized in that: The free radical photoinitiator is one or more of benzoin, benzoin ether, acetophenone, and acetophenone ketal compounds; the cationic photoinitiator is one or more of diaryl iodonium salt, triaryl sulfonium salt, and alkyl sulfonium salt compounds.

8. A low warping and scratch-resistant matt film, characterized in that: It comprises a coating and a film layer; the coating is formed by coating the low warping and scratch-resistant matte coating as described in any one of claims 1 to 7 on the surface of the film layer; the film layer is a BOPP film layer.

9. The low warping and scratch-resistant matt film according to claim 8, characterized in that: The dry weight of the coating is 1-4 g / m 2 ; The thickness of the BOPP film layer is 8-12μm.

10. A method for preparing a low warping and scratch-resistant matt film according to claim 8 or 9, characterized in that: The following steps are involved: S1: preparing the low warpage and scratch-resistant matte coating according to any one of claims 1 to 7; S2: coating the low warpage and anti-scratch matte coating on the surface of the BOPP film, drying the solvent, and curing with ultraviolet light to obtain the low warpage and anti-scratch matte film.