Modified nitrile rubber-based conductive glue, glue film and preparation method thereof
The prepolymerization reaction of conductive metal filler and nitrile rubber matrix forms a semi-cured conductive glue or adhesive film, which solves the problems of early curing and poor weather resistance of existing conductive glues, and achieves high-performance and low-cost conductive glue preparation.
Patent Information
- Application Number
- CN202411172156.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-11-08
AI Technical Summary
Existing conductive glues are prone to cure in advance before use or during use, resulting in inconvenient use, short shelf life and poor weather resistance, and high cost.
The preparation method of modified nitrile rubber-based conductive glue is adopted to form a semi-cured glue or glue film through the prepolymerization reaction between conductive metal fillers and nitrile rubber matrix, and combined with functional additives to enhance the chemical bond between molecules and extend the Shelf life and reduce costs.
The weather resistance and conductivity of conductive glue and film are significantly improved, the shelf life is extended, the production cost is reduced, and the accuracy and stability of the glue coating position are improved.
Smart Images

Figure BDA0005009608980000031 
Figure BDA0005009608980000032 
Figure BDA0005009608980000041
Abstract
Description
Technical Field
[0001] The invention relates to a conductive glue, a glue film and a preparation method thereof, in particular to a modified nitrile rubber conductive glue, a glue film and a preparation method thereof, and belongs to the field of microelectronic packaging connection materials. Background Art
[0002] Conductive glue is an adhesive that has a certain degree of conductivity after curing or drying. It can connect a variety of conductive materials together to form an electrical path between the connected materials. In the electronics industry, conductive glue has become an indispensable new material.
[0003] There are many types of conductive glue, and from the perspective of application, conductive glue can be divided into two categories: general conductive glue and special conductive glue. General conductive glue only has certain requirements for conductivity and bonding strength, while special conductive glue has other special requirements in addition to certain requirements for conductivity and bonding strength, such as high temperature resistance, ultra-low temperature resistance, instant curing, anisotropy and transparency, etc.
[0004] Conductive glue is mainly composed of resin matrix, conductive particles and other additives. The resin matrix generally selects various types of polymer resins with good viscosity, among which the most widely used is epoxy resin matrix. Due to its thermosetting and adhesive properties, as well as the convenience of modification or use as a modification of other materials, it is widely applicable for the ingredients of conductive glue with special requirements. In addition, conductive glue requires that the conductive particles themselves have good conductivity and the particle size should be within a suitable range, and can be added to the conductive glue matrix to form a conductive path. Conductive fillers can be gold, silver, copper, aluminum, zinc, iron, nickel powder and graphite and some conductive compounds.
[0005] Most of the conductive glues on the market are based on epoxy resin systems, and the curing conditions of using this system rely on epoxy resin curing agents. The addition of epoxy resin curing agents can easily cause the epoxy resin system in the conductive glue to cure before use, which greatly reduces the shelf life of the glue / film, causes poor weather resistance, is inconvenient to use, is easy to flow, and causes inaccurate glue coating positions. The use of imported high-quality curing agents or resins is expensive.
[0006] The nitrile rubber-based conductive glue of the present invention has created a new type of curing system, which uses the conductive filler itself and the glue system to undergo prepolymerization reaction (i.e., the metal conductive filler particles themselves and the nitrile rubber-based matrix glue first undergo prepolymerization reaction), and after being made into semi-cured glue or glue film, other additives (i.e., functional additives, acrylate rubber, curing agent, accelerator, coupling agent, inhibitor) are combined to ensure the convenience of use of the product and extend the shelf life of the product. The glue of the present invention is stirred, and the mixed raw materials undergo prepolymerization reaction, and the conductive metal filler and the matrix glue undergo a certain degree of coordination and complexation reaction to form a chemical bond that enhances the stability of the overall product structure, which not only ensures the convenience of use and the shelf life of the product; the fluidity of the prepolymerized and cross-linked glue is reduced, and the semi-cured glue or glue film formed is not easy to have the phenomenon of glue flow during use, and the glue coating position is accurate during the glue coating process; and the glue after prepolymerization and cross-linking has a certain stable structure, and the glue and glue film are less susceptible to environmental factors when stored. Moreover, for some conductive glues or films with special requirements, such as excellent high temperature resistance, the coordination prepolymerization reaction between the conductive filler and the glue itself can greatly enhance the intermolecular force, so that the weather resistance of the cured product can be significantly improved, thereby replacing the use of some expensive special materials, such as modified epoxy resins containing polyaromatic groups, high temperature resistant modified polyurethanes, and amide resins modified with ring structures as resin matrices, thereby reducing market costs.
[0007] In the preparation process of the conductive glue or adhesive film of the present invention, before the conductive metal filler is added, the matrix raw material and the functional additive undergo a prepolymerization crosslinking reaction during the stirring and blending process to form a semi-cured glue. The substances undergo a chemical reaction to form bonds, the intermolecular force is enhanced, the overall structure and properties of the adhesive film are more stable, and compared with the case where there is no chemical reaction between the raw materials and simple physical mixing, it is less likely to change when facing the influence of external environmental factors, and the performance is comprehensively improved. Summary of the invention
[0008] The present invention aims at the technical defects of the conductive glue / film of connection materials in the existing microelectronic packaging field, such as weak intermolecular interaction force and poor weather resistance; and the glue is cured in advance before or during use, resulting in inconvenient product use and short shelf life. The present invention provides a modified nitrile rubber-based conductive glue / film and a preparation method thereof. The conductive glue / film prepared by the method of the present invention has innovative curing technology, significantly enhanced intermolecular interaction force, high peel strength, and significantly improved weather resistance of the cured product. The product has low resistance and high conductivity. In addition, the conductive glue and film prepared by the method of the present invention have low cost and simple process.
[0009] To achieve the purpose of the present invention, the present invention adopts the following technical solutions:
[0010] A method for preparing a modified nitrile rubber-based conductive adhesive comprises the following steps in order:
[0011] 1) stirring and mixing the raw materials of nitrile rubber, solvent, bisphenol A epoxy resin, phenolic resin, polyimide and / or bismaleimide to obtain a nitrile rubber solution, i.e., obtaining solution A;
[0012] 2) Under stirring, adding functional additives to solution A in sequence, stirring and mixing evenly to obtain a matrix glue;
[0013] 3) Adding metal conductive filler into the base glue under stirring to obtain nitrile rubber-based conductive glue.
[0014] Wherein, the weight proportion of the raw materials nitrile rubber, solvent, bisphenol A epoxy resin, phenolic resin, polyimide and / or bismaleimide in step 1) is:
[0015]
[0016] In particular, the weight ratio of the raw materials nitrile rubber, ketone solvent, bisphenol A epoxy resin, phenolic resin, polyimide and / or bismaleimide is preferably:
[0017]
[0018] In particular, the weight ratio of the raw material polyimide and / or bismaleimide is preferably 5.
[0019] Particularly, when polyimide and bismaleimide are selected from the raw materials, the sum of their weight parts is 5, wherein the weight ratio of polyimide to bismaleimide is 2:3.
[0020] In particular, the solvent in step 1) is one or more of toluene, acetone, butanone, cyclohexanone, ethyl acetate, and butyl acetate, preferably butanone.
[0021] In particular, the epoxy equivalent of the bisphenol A epoxy resin is greater than 500 g / mol, preferably 500-600 g / mol, and more preferably 600 g / mol.
[0022] In particular, the phenolic resin is a conventional thermosetting phenolic resin; the softening point of the phenolic resin is 80-90° C.; and the hydroxyl equivalent is 100-110 g / eq.
[0023] In particular, the polyimide and bismaleimide are ketone-soluble polycondensation-type polyimide; the viscosity is 1200-2000 (25° C., mPa.s), preferably 1500±50 mPa.s.
[0024] In particular, the stirring rate in step 1) is ≥500 rpm, preferably 500-1200 rpm; and the stirring time is 0.5-1 h.
[0025] In particular, the functional additive in step 2) is one or more of acrylic rubber, curing agent, accelerator, coupling agent and inhibitor.
[0026] In particular, the functional additives are acrylic rubber, curing agent, accelerator, coupling agent and inhibitor.
[0027] In particular, the weight ratio of the functional additive is:
[0028]
[0029] In particular, the weight ratio of the functional additive is preferably:
[0030]
[0031] In particular, the acrylic rubber has an acid value greater than 50 (KOH) / (mg / g), preferably 50-60 (KOH) / (mg / g); and a molecular weight greater than 1000 Da, preferably 1000-1500 Da.
[0032] In particular, the curing agent is hexamethylenetetramine, dinitrile amine, methylhexahydrophthalic anhydride, or imidazole with alkane-substituted groups.
[0033] In particular, the imidazole with an alkane-substituted group is 2-methylimidazole, 2-propylimidazole, 2-isopropylimidazole, or dodecaneimidazole.
[0034] In addition to 2-methylimidazole, other imidazoles with alkane substituents, hexamethylenetetramine, methylhexahydrophthalic anhydride, dicyandiamide, are suitable for the present invention, and other imidazoles with alkyl substituents such as 2-propylimidazole, 2-isopropylimidazole, dodecaneimidazole
[0035] In particular, the accelerator is triphenylphosphine, a tertiary amine salt, a substituted urea, a carboxylic acid metal salt or a phenol.
[0036] In particular, the tertiary amine salt is N,N-dimethylcyclohexylamine, triethylamine or N,N-dimethylaniline; the substituted urea is GLOC-500; and the carboxylic acid metal salt is one or more of copper acetate, sodium acetate or sodium benzoate.
[0037] In particular, the coupling agent is a silane coupling agent, such as silane coupling agent KH560, KH550, KH570.
[0038] In particular, the inhibitor is one or more of antioxidant 1010, antioxidant 1076, diphenylamine, p-diphenylamine, and butylated hydroxytoluene, preferably butylated hydroxytoluene, antioxidant 1010, and antioxidant 1076.
[0039] In particular, the stirring rate in step 2) is ≥500 rpm, preferably 500-1200 rpm; the stirring time is at least 5 min, preferably 5-15 min.
[0040] In particular, the weight ratio of the metal conductive filler added in step 3) is 20-35, preferably 25-28.
[0041] In particular, the metal conductive filler is one or more of nickel powder, copper powder, silver powder, gold powder, silver-coated copper powder, silver-coated nickel powder, gold-coated nickel powder, nickel-coated glass microspheres, copper-coated glass microspheres, silver-coated glass microspheres, and graphite powder, preferably copper powder, silver-coated copper powder, or silver-coated nickel powder.
[0042] In particular, in step 3), the stirring rate is ≥500 rpm, preferably 500-1200 rpm; and the stirring time is continued for at least 20 min, preferably 20-30 min, after adding the metal conductive filler.
[0043] In particular, the method further comprises storing the prepared nitrile rubber-based conductive glue in a low temperature environment of 2-10°C.
[0044] Another technical solution of the present invention is as follows: providing a modified nitrile rubber-based conductive glue prepared according to the above method.
[0045] Another technical solution of the present invention is as follows: A method for preparing a modified nitrile rubber-based conductive film, comprising the following steps in order:
[0046] A) stirring and mixing nitrile rubber, ketone solvent, bisphenol A type epoxy resin, phenolic resin, polyimide and / or bismaleimide to obtain a nitrile rubber solution, i.e., obtaining solution A;
[0047] B) adding functional additives to solution A in sequence under stirring, stirring and mixing evenly to obtain a matrix glue;
[0048] C) adding a metal conductive filler to the base glue under stirring to obtain a nitrile rubber-based conductive glue;
[0049] D) The conductive glue is coated on the release film, followed by drying, drying the solvent to form a film, and then curing to obtain a conductive adhesive film.
[0050] In particular, in step D), the coating temperature is 85-160°C; the drying temperature is 80-130°C; the drying time is 2-5 minutes; the curing temperature is 35-45°C; and the curing time is 24-48 hours.
[0051] Another technical solution of the present invention is as follows: providing a modified nitrile rubber-based conductive adhesive film prepared according to the above method.
[0052] Compared with the prior art, the present invention has the following advantages and benefits:
[0053] 1. The modified nitrile rubber base system and the functional additives in the conductive glue / film of the present invention form chemical bonds and intermolecular forces through coordination prepolymerization reaction and coordination complexation, that is, the semiconductor polymer nitrile rubber and the metal conductive filler form chemical bonds through hole-electron pair coordination complexation, so as to obtain glue and film in a semi-cured state, so that the conductive filler and the base glue are more tightly combined, the conductive filler is more evenly dispersed, and can remain stable for a long time, which greatly improves the shelf life of the product, avoids the selection of high-cost curing materials, and significantly reduces the production cost.
[0054] 2. The curing system adopted in the present invention is adapted to the application requirements of special conductive glue or conductive adhesive film. The resins of traditional curing systems mostly rely on expensive ones, such as modified epoxy resins containing polyaromatic groups, high temperature resistant modified polyurethanes, special resins such as amide resins modified by introducing ring structures, and special curing agents such as end-capped amine curing agents. The curing method adopted in the present invention utilizes the chemical properties between conventional base materials such as nitrile rubber, bisphenol A epoxy resin, and acrylate rubber, and uses ordinary resins with cost advantages to modify and coordinate them, so that the glue matrix itself and the conductive filler are truly combined into the same composite material, not just physically fused. Therefore, the overall material performance is stable and can meet the requirements in extreme environments and special needs.
[0055] 3. In the process of preparing the conductive glue / film by the method of the present invention, the base glue and the conductive filler participate in a chemical reaction, the length and strength of the formed chemical bonds are consistent, and the conductive filler is evenly dispersed in the glue / film, thereby improving the uniformity and stability of the conductive performance.
[0056] 4. The conductive glue prepared by the method of the present invention has strong viscosity and high peel strength: the materials in the modified nitrile rubber used in the base glue, whether it is nitrile rubber itself or other resins, have high viscosity. Nitrile rubber, phenolic resin, bisphenol A epoxy resin and functional additives are mixed. After modification and combination, chemical bonds are formed between the resins through conductive fillers as bridges, among which the chemical functional groups that provide bonding properties have a higher density and interact with each other to make the viscosity stronger.
[0057] 5. The conductive adhesive film prepared by the method of the present invention has excellent heating and re-adhesive properties: In the application field of the conductive adhesive film, it is necessary to ensure that the adhesive film has sufficient re-adhesive properties during use so that components can be well bonded. The base glue material used in the present invention selects some materials with low glass transition temperature such as traditional nitrile rubber, bisphenol A epoxy resin, and phenolic resin, so it has a strong ability to soften and re-adhere when heated.
[0058] 6. The conductive adhesive film prepared by the method of the present invention has good high temperature and high humidity resistance: the curing method of the present invention, which relies on the conductive filler as a bridge to produce a coordination reaction with the base glue, determines that the base material does not need to add a large amount of high temperature resistant materials that are easy to destroy the back adhesion. The large number of stable chemical bonds inside the material itself are used to form extremely strong heat shock resistance, and the dense chemical molecular structure after complete curing is sufficient to resist the erosion of water vapor, and can be used in many extreme environments.
[0059] The conductive adhesive film of the present invention has good conductivity, small resistance change rate, high peel strength, excellent high temperature resistance and moisture and heat resistance, good operating performance, and can be stored at room temperature for more than 60 days. DETAILED DESCRIPTION
[0060] The present invention will be further described below in conjunction with specific embodiments, and the advantages and features of the present invention will become clearer as the description proceeds. However, these embodiments are exemplary only and do not constitute any limitation to the scope of the present invention. It should be understood by those skilled in the art that the details and forms of the technical solution of the present invention may be modified or replaced without departing from the spirit and scope of the present invention, but these modifications and replacements all fall within the scope of protection of the present invention.
[0061] Example 1: Preparation of conductive glue
[0062] 1. Prepare nitrile rubber solution (i.e. prepare solution A)
[0063] 1A) Prepare the following raw materials by weight (×10 g):
[0064]
[0065] Among them, the ketone solvent is butanone; the epoxy equivalent of bisphenol A epoxy resin is 600g / mol (usually greater than 500g / mol, preferably 500-600g / mol); the phenolic resin is a conventional thermosetting phenolic resin with a softening point of 80-90°C and a hydroxyl equivalent of 100-110g / eq; and the polyimide is a ketone-soluble condensation polyimide with a viscosity of 1500±50mPa.s (usually 1200-2000mPa.s).
[0066] In this embodiment, butanone is used as an example to illustrate the ketone solvent, and other ketone solvents such as acetone and cyclohexanone are also applicable to the present invention.
[0067] The bisphenol A type epoxy resin is an epoxy resin with an epoxy equivalent greater than 500 g / mol; the phenolic resin is a thermosetting phenolic resin with a softening point of 80-90° C. and a hydroxyl equivalent of 100-110 g / eq; and the polyimide is a ketone-soluble polycondensation type polyimide with a viscosity of 1200-2000 mPa.s, all of which are suitable for the present invention.
[0068] In addition to polyimide, bismaleimide is also suitable for the present invention, and both can improve the high temperature resistance and mechanical properties of the glue product.
[0069] 1B) Under stirring, acrylonitrile butadiene rubber, ketone solvent, bisphenol A epoxy resin, phenolic resin and polyimide are stirred and mixed uniformly to obtain acrylonitrile butadiene rubber solution (i.e., solution A) for standby use, wherein the stirring rate is 1000±50rpm (usually ≥500rpm); the stirring time is 0.5h (usually 0.5-1h);
[0070] 2. Prepare functional additives according to the following ratio (i.e. prepare component B, × 10g)
[0071]
[0072] The curing agent is 2-methylimidazole; the accelerator is triphenylphosphine; the coupling agent is silane coupling agent KH560; the inhibitor is butylated hydroxytoluene; the metal conductive filler is silver-coated copper powder;
[0073] In addition to 2-methylimidazole, the curing agent includes other imidazoles with alkane substituents, hexamethylenetetramine, methylhexahydrophthalic anhydride, dicyandiamide, etc., which are suitable for the present invention. Other imidazoles with alkyl substituents include 2-propyl imidazole, 2-isopropyl imidazole, and dodecane imidazole.
[0074] In addition to triphenylphosphine, other accelerators such as tertiary amine salts, substituted ureas, carboxylic acid metal salts, and phenol are all suitable for the present invention, wherein the tertiary amine salts include N, N-dimethylcyclohexylamine, triethylamine, N, N-dimethylaniline, etc.; the substituted urea is GLOC-500; the carboxylic acid metal salts are cupric acetate, sodium acetate, and sodium benzoate.
[0075] In addition to the silane coupling agent KH560, other silane coupling agents in the art are suitable for the present invention, such as KH550 and KH570;
[0076] In addition to butylated hydroxytoluene, other inhibitors such as antioxidant 1010, antioxidant 1076, diphenylamine, and p-diphenylamine are all suitable for the present invention.
[0077] In addition to silver-coated copper powder, other metal conductive fillers such as nickel powder, copper powder, silver powder, gold powder, silver-coated copper powder, silver-coated nickel powder, gold-coated nickel powder, nickel-coated glass microspheres, copper-coated glass microspheres, silver-coated glass microspheres, and conductive non-metals are suitable for the present invention, preferably copper powder, nickel powder, silver-coated copper powder, and silver-coated nickel powder. If multiple metal fillers are mixed and used, they can be mixed in any proportion. The proportion can be changed according to the change in the price cost of the metal raw material, the conductivity requirement, or the color change required by the glue. Conductive non-metals such as graphite powder, sintered graphene powder or carbon black.
[0078] 3. Under stirring, add the other additives (acrylate rubber, curing agent, accelerator, silane coupling agent, inhibitor) in step 2) except the metal conductive filler to the solution A prepared in step 1) in sequence, wherein the order of addition is acrylate rubber, curing agent, accelerator, silane coupling agent, inhibitor, and the stirring rate is 1000 rpm (usually ≥500 rpm, preferably 500-1000 rpm);
[0079] First, an acrylate resin providing a reactive carboxylic acid group is added to carry out subsequent prepolymerization cross-linking reaction and coordination reaction. At the same time, it also acts as an auxiliary dispersant, so that the curing agent, accelerator, silane coupling agent, and inhibitor are fully dispersed, thereby improving the dispersion uniformity and reaction uniformity.
[0080] 4. After adding the auxiliary raw materials except the metal conductive filler in sequence, continue stirring for 10 minutes (usually 5-15 minutes) to obtain a base glue; then add the metal conductive filler to the base glue under stirring, continue stirring for 25 minutes (usually at least 20 minutes, preferably 20-30 minutes), stir and mix evenly, and obtain the modified nitrile rubber conductive glue of the present invention;
[0081] The first stirring when adding the functional additives other than the metal conductive filler in step 4) ensures that the glue raw materials are fully mixed, and the acrylic rubber raw materials therein provide a dispersing effect and an acidic environment;
[0082] The second stirring treatment after adding the metal conductive filler is conducive to the full mixing of the metal conductive filler in the base glue, and the coordination complex reaction occurs under acidic conditions; under the acidic environment, the carboxylate and the positively charged metal ions undergo a coordination complex reaction to form chemical bonds. Due to the effect of the inhibitor, this coordination complex reaction is controlled to a certain extent, ensuring that only a small part of the metal filler is oxidized to provide an enhancement effect on the overall physical and chemical stability of the glue, retaining most of the unoxidized parts to continue to provide conductivity.
[0083] The chemical reaction is a redox reaction between the carboxyl groups provided by the acrylic rubber with an acid value and the metal filler. Under the action of the inhibitor, only a small part of the metal is oxidized to produce a coordination complex bond between the carboxylate and the metal cation, thereby improving the performance stability and weather resistance of the conductive glue or film, extending the shelf life of the glue / film, etc. Increasing the chemical bond content between the ingredients helps to improve the stability and weather resistance of the product, and is not easy to fail or expire due to environmental and time factors.
[0084] 5. Transfer the prepared modified nitrile rubber conductive glue into a glue barrel, cover it with a lid and seal it with adhesive tape, and then store it in a low temperature environment of 2-10°C for future use. The conductive glue prepared by the present invention contains a rubber material with a relatively low TG point, and the rubber material is prone to aging. Storing it in the range of 2-10°C can significantly reduce the aging speed of the rubber and ensure that other materials are not inactivated.
[0085] Example 1A: Preparation of conductive adhesive film
[0086] The conductive glue prepared in Example 1 is coated on the release film by a coater, wherein the coater temperature is 100°C (usually 85-160°C); the coating thickness is 60 μm (usually 50-70 μm); then a drying treatment is performed to dry the solvent to form a film, wherein the drying tunnel temperature is controlled to be 100°C (usually 80-130°C); the drying is performed for 5 minutes (usually 2-5 minutes); the film is rolled up and placed in a drying room at 35-45°C for curing for 24-48 hours to obtain a conductive film.
[0087] Example 2: Preparation of conductive glue
[0088] 1. Prepare nitrile rubber solution (i.e. prepare solution A)
[0089] 1A) Prepare the following raw materials by weight (×10 g):
[0090]
[0091] Among them, the ketone solvent is butanone; the epoxy equivalent of bisphenol A epoxy resin is 600g / mol (usually greater than 500g / mol, preferably 600g / mol); the phenolic resin is a conventional thermosetting phenolic resin with a softening point of 80-90°C and a hydroxyl equivalent of 100-110g / eq; and the viscosity of bismaleimide is 1500±50mPa.s (usually 1200-2000mPa.s).
[0092] 1B) Under stirring, acrylonitrile butadiene rubber, ketone solvent, bisphenol A epoxy resin, thermosetting phenolic resin and bismaleimide are stirred and mixed uniformly to obtain acrylonitrile butadiene rubber solution (i.e., solution A) for standby use, wherein the stirring rate is 1000±50rpm (usually ≥500rpm); the stirring time is 0.5h (usually 0.5-1h);
[0093] Epoxy resin and phenolic resin are thermosetting resins. After thermosetting, the viscosity is enhanced, which improves the stability of the product. This product is a glue and film used under thermosetting conditions.
[0094] 2. Prepare functional additives according to the following ratio (i.e. prepare component B, × 10g)
[0095]
[0096] The curing agent is methyl hexahydrophthalic anhydride; the accelerator is triethylamine; the coupling agent is silane coupling agent KH550; the inhibitor is antioxidant 1010; the metal conductive filler is copper powder;
[0097] In addition to methyl hexahydrophthalic anhydride, other curing agents such as dicyandiamide, hexamethylenetetramine, and imidazoles with alkane-substituted groups are suitable for the present invention, wherein the imidazoles with alkane-substituted groups are such as 2-methylimidazole, 2-propylimidazole, 2-isopropylimidazole, and dodecaneimidazole;
[0098] In addition to triethylamine, other accelerators such as triphenylphosphine, tertiary amine salts, substituted ureas, carboxylic acid metal salts, and phenol are all suitable for the present invention, wherein the tertiary amine salts include N, N-dimethylcyclohexylamine, triethylamine, N, N-dimethylaniline, etc.; the substituted urea is GLOC-500; and the carboxylic acid metal salts are cupric acetate, sodium acetate, and sodium benzoate.
[0099] In addition to the silane coupling agent KH550, other silane coupling agents in the art are suitable for the present invention, such as KH560 and KH570;
[0100] In addition to antioxidant 1010, other inhibitors such as antioxidant 1076, butylated hydroxytoluene, diphenylamine, and p-diphenylamine are also suitable for the present invention.
[0101] In addition to nickel powder, copper powder, and silver-coated copper, other metal conductive fillers such as gold, silver, aluminum, zinc, iron, silver-coated nickel powder, and one or more mixtures of conductive non-metals are suitable for the present invention, and conductive non-metals such as graphite powder, sintered graphene powder or carbon black.
[0102] The functions of the functional additives in the method of the present invention are as follows: the acrylic rubber provides acidic group carboxyl and increases the acid value of the product, promoting and participating in the coordination and complexation with the subsequent metal conductive filler particles; when the conductive glue product is in the use state, the curing agent undergoes a curing reaction with the double A-type epoxy resin after being subjected to hot pressing to cure the epoxy resin; the role of the accelerator is to promote the curing effect of the curing agent; the coupling agent is used to increase the connectivity of different polymer materials and conductive metal fillers; the inhibitor ensures that the product does not react with the curing agent before being subjected to the hot pressing process and entering the use state (the use state refers to the process before the glue and the film are subjected to hot pressing curing, and the inhibitor has a second function besides ensuring that the metal conductive fillers do not all undergo complexation reaction) to increase the shelf life.
[0103] Component B is a functional additive. The raw materials are divided into solution A and component B for uniform dispersion. If the curing agent, accelerator and other functional additives are not added together with the inhibitor, there is a possibility of premature reaction during the stirring process, which will affect the product production.
[0104] 3. Under stirring, add the other additives (acrylate rubber, curing agent, accelerator, silane coupling agent, inhibitor) except the metal conductive filler in step 2) to the solution A prepared in step 1) in sequence, wherein the order of addition is acrylate rubber, methyl hexahydrophthalic anhydride, triethylamine accelerator, silane coupling agent KH550, antioxidant 1010; the stirring rate is 1000 rpm (usually ≥500 rpm);
[0105] 4. After adding the additives except the metal conductive filler in sequence, continue stirring for 10 minutes (usually at least 5 minutes, preferably 5-15 minutes) to obtain a base glue; then add the metal conductive filler to the base glue under stirring, continue stirring for 25 minutes (usually at least 20 minutes, preferably 20-30 minutes), stir and mix evenly, and obtain the modified nitrile rubber conductive glue of the present invention;
[0106] 5. Transfer the prepared modified nitrile rubber conductive glue into a glue barrel, cover it with a lid and seal it with adhesive tape, and then place it in a low temperature environment of 2-10°C (usually 2-10°C) for storage. The conductive glue prepared by the present invention contains a rubber material with a relatively low TG point, and the rubber material is easy to age. Storing it in the range of 2-10°C can significantly reduce the aging speed of the rubber and ensure that other materials are not inactivated.
[0107] Example 2A: Preparation of conductive adhesive film
[0108] The conductive glue prepared in Example 2 is coated on the release film by a coater, wherein the coater temperature is 100°C (usually 85-160°C); the coating thickness is 50μm (usually 50-70μm); then a drying treatment is performed to dry the solvent to form a film, wherein the drying tunnel temperature is controlled to be 100°C (usually 80-130°C); drying is performed for 2min (usually 2-5min); the solvent is dried to form a film, which is rolled up and placed in a drying room at 35-45°C for curing for 24-48 hours to obtain a conductive adhesive film.
[0109] Example 3: Preparation of conductive glue
[0110] 1. Prepare nitrile rubber solution (i.e. prepare solution A)
[0111] 1A) Prepare the following raw materials by weight (×10 g):
[0112]
[0113]
[0114] Among them, the ketone solvent is butanone; the epoxy equivalent of bisphenol A epoxy resin is 600g / mol (usually greater than 500g / mol, preferably 600g / mol); the phenolic resin is a conventional thermosetting phenolic resin with a softening point of 80-90°C and a hydroxyl equivalent of 100-110g / eq; the polyimide is a ketone-soluble condensation polyimide with a viscosity of 1500±50mPa.s (usually 1200-2000mPa.s).
[0115] 1B) stirring and mixing the nitrile rubber, ketone solvent, bisphenol A epoxy resin, thermosetting phenolic resin and polycondensation polyimide to obtain a modified nitrile rubber solution (i.e., solution A) for standby use, wherein the stirring rate is 1000±50 rpm and the stirring time is 0.5 h;
[0116] 2. Prepare functional additives according to the following ratio (i.e. prepare component B, × 10g)
[0117]
[0118] The curing agent is dicyandiamide; the accelerator is triethylamine; the coupling agent is silane coupling agent KH560; the inhibitor is antioxidant 1076; the metal conductive filler is nickel powder;
[0119] In addition to dicyandiamide, other curing agents such as methyl hexahydrophthalic anhydride, hexamethylenetetramine, and imidazoles with alkane-substituted groups are suitable for the present invention, wherein the imidazoles with alkane-substituted groups are such as 2-methylimidazole, 2-propylimidazole, 2-isopropylimidazole, and dodecaneimidazole;
[0120] In addition to triethylamine, other accelerators such as triphenylphosphine, tertiary amine salts, substituted ureas, carboxylic acid metal salts, and phenol are all suitable for the present invention, wherein the tertiary amine salts include N, N-dimethylcyclohexylamine, triethylamine, N, N-dimethylaniline, etc.; the substituted urea is GLOC-500; and the carboxylic acid metal salts are cupric acetate, sodium acetate, and sodium benzoate.
[0121] In addition to the silane coupling agent KH560, other silane coupling agents in the art are suitable for the present invention, such as KH550 and KH570;
[0122] Inhibitors, in addition to antioxidant 1076, butylated hydroxytoluene, antioxidant 1010, diphenylamine, p-diphenylamine, etc. are all suitable for the present invention;
[0123] 3. Under stirring, add the acrylic rubber, dicyandiamide, triethylamine accelerator, silane coupling agent KH560 and antioxidant 1076 prepared in step 2) to the solution A prepared in step 1) in sequence, with a stirring rate of 1000 rpm (usually ≥500 rpm);
[0124] 4. After adding the auxiliary raw materials except the metal conductive filler in sequence, continue stirring for 5 minutes to obtain the base glue; then add the metal conductive filler to the base glue under stirring, continue stirring for 30 minutes, stir and mix evenly, and obtain the modified nitrile rubber conductive glue of the present invention;
[0125] 5. Transfer the prepared modified nitrile rubber conductive glue into a rubber barrel, cover it with a lid and seal it with tape, then store it in a low temperature environment of 2-10°C for future use.
[0126] Example 3A: Preparation of conductive adhesive film
[0127] The conductive glue prepared in Example 3 is coated on the release film by a coater, wherein the coater temperature is 100°C (usually 85-160°C); the coating thickness is 70μm (usually 50-70μm); then a drying treatment is performed, wherein the drying tunnel temperature is controlled to be 100°C (usually 80-130°C); drying is performed for 5 minutes; the solvent is dried to form a film, which is rolled up and placed in a drying room at 35-45°C for curing for 24-48 hours to obtain a conductive adhesive film.
[0128] Example 4: Preparation of conductive glue
[0129] 1. Prepare nitrile rubber solution (i.e. prepare solution A)
[0130] 1A) Prepare the following raw materials by weight (×10 g):
[0131]
[0132] Among them, the ketone solvent is butanone; the epoxy equivalent of bisphenol A epoxy resin is 600g / mol (usually greater than 500g / mol, preferably 600g / mol); the phenolic resin is a conventional thermosetting phenolic resin with a softening point of 80-90°C and a hydroxyl equivalent of 100-110g / eq; and the viscosity of bismaleimide is 1500±50mPa.s (usually 1200-2000mPa.s).
[0133] 1B) stirring and mixing the nitrile rubber, ketone solvent, bisphenol A epoxy resin, thermosetting phenolic resin and bismaleimide to obtain a modified nitrile rubber solution (i.e., solution A) for standby use, wherein the stirring rate is 1000±50 rpm and the stirring time is 1 hour;
[0134] 2. Prepare functional additives according to the following ratio (i.e. prepare component B, × 10g)
[0135]
[0136] Wherein, the curing agent is hexamethylenetetramine; the accelerator is triethylamine; the coupling agent is silane coupling agent KH550; the inhibitor is antioxidant 1010; the metal conductive filler is a mixture of silver-coated copper powder, copper powder, and nickel powder (mass ratio of 1:2:3) (the three can be mixed in any proportion);
[0137] In addition to hexamethylenetetramine, curing agents such as dicyandiamide, methyl hexahydrophthalic anhydride, and imidazoles with alkane substituents are all suitable for the present invention, wherein imidazoles with alkane substituents are such as 2-methylimidazole, 2-propylimidazole, 2-isopropylimidazole, and dodecane imidazole; in addition to triethylamine, accelerators such as triphenylphosphine, tertiary amine salts, substituted ureas, carboxylic acid metal salts, and phenol are all suitable for the present invention, wherein the tertiary amine salts are such as N, N-dimethylcyclohexylamine, triethylamine, and N, N-dimethylaniline; the substituted urea is GLOC-500; the carboxylic acid metal salts are copper acetate, sodium acetate, and sodium benzoate. In addition to silane coupling agent KH550, other silane coupling agents in the art are all suitable for the present invention, such as KH560 and KH570; in addition to antioxidant 1010, inhibitors such as antioxidant 1076, butylated hydroxytoluene, diphenylamine, and p-diphenylamine are all suitable for the present invention. In addition to nickel powder, copper powder, and silver-coated copper, other metal conductive fillers such as gold, silver, aluminum, zinc, iron, silver-coated nickel powder, and one or more mixtures of conductive non-metals are suitable for the present invention, and conductive non-metals such as graphite powder, sintered graphene powder or carbon black.
[0138] 3. Under stirring, add the other additives (acrylate rubber, curing agent, accelerator, silane coupling agent, inhibitor) except the metal conductive filler in step 2) to the solution A prepared in step 1) in sequence, wherein the order of addition is acrylate rubber, hexamethylenetetramine, triethylamine accelerator, silane coupling agent KH550, antioxidant 1010; the stirring rate is 1000 rpm (usually ≥500 rpm);
[0139] 4. After adding the additives except the metal conductive filler in sequence, continue stirring for 10 minutes to obtain a base glue; then add the metal conductive filler to the base glue under stirring, continue stirring for 25 minutes, and stir and mix evenly to obtain the modified nitrile rubber conductive glue of the present invention;
[0140] 5. Transfer the prepared modified nitrile rubber conductive glue into a rubber barrel, cover it with a lid and seal it with tape, then store it in a low temperature environment of 2-10°C for future use.
[0141] Example 4A: Preparation of conductive adhesive film
[0142] The conductive glue prepared in Example 4 is coated on the release film by a coater, wherein the coater temperature is 100°C (usually 85-160°C); the coating thickness is 60μm (usually 50-70μm); then a drying treatment is performed, wherein the drying tunnel temperature is controlled to be 100°C (usually 80°C~130°C); the solvent is dried to form a film, which is rolled up and placed in a drying room at 35~45°C for curing for 24~48 hours to obtain a conductive adhesive film.
[0143] Example 5: Preparation of conductive glue
[0144] 1. Prepare nitrile rubber solution (i.e. prepare solution A)
[0145] 1A) Prepare the following raw materials by weight (×10 g):
[0146]
[0147] Wherein, the ketone solvent is butanone; the epoxy equivalent of bisphenol A epoxy resin is 600g / mol (usually greater than 500g / mol, preferably 600g / mol); the phenolic resin is a conventional thermosetting phenolic resin with a softening point of 80-90°C and a hydroxyl equivalent of 100-110g / eq; the viscosity of bismaleimide is 1500±50mPa.s (usually 1200-2000 (25°C, mPa.s); the viscosity of polyimide is 1500±50mPa.s (usually 1200-2000 (25°C, mPa.s).
[0148] 1B) Under stirring, acrylonitrile-butadiene rubber, ketone solvent, bisphenol A epoxy resin, thermosetting phenolic resin, bismaleimide and polyimide are stirred and mixed uniformly to obtain a modified acrylonitrile-butadiene rubber solution (i.e., solution A) for standby use, wherein the stirring rate is 1000±50rpm (usually ≥500rpm); the stirring time is 0.5h (usually 0.5-1h);
[0149] 2. Prepare functional additives according to the following ratio (i.e. prepare component B, × 10g)
[0150]
[0151] The curing agent is dicyandiamide; the accelerator is triethylamine; the coupling agent is silane coupling agent KH560; the inhibitor is antioxidant 1010; the metal conductive filler is a mixture of silver-coated copper powder, copper powder and nickel powder mixed in a ratio of 1:1:1 (mass ratio);
[0152] In addition to dicyandiamide, other curing agents such as methyl hexahydrophthalic anhydride, hexamethylenetetramine, and imidazoles with alkane-substituted groups are all suitable for the present invention, wherein the imidazoles with alkane-substituted groups include 2-methylimidazole, 2-propylimidazole, 2-isopropylimidazole, and dodecaneimidazole; in addition to triethylamine, other accelerators such as triphenylphosphine, tertiary amine salts, substituted ureas, carboxylic acid metal salts, and phenol are all suitable for the present invention, wherein the tertiary amine salts include N,N-dimethylcyclohexylamine, triethylamine, N,N-dimethylaniline, etc.; the substituted urea is GLOC-500; the carboxylic acid metal salts are cupric acetate, sodium acetate, and sodium benzoate. In addition to the silane coupling agent KH560, other silane coupling agents in the art are applicable to the present invention, such as KH550 and KH570; in addition to the antioxidant 1076, the inhibitors such as butylated hydroxytoluene, antioxidant 1010, diphenylamine, and p-diphenylamine are applicable to the present invention; in addition to nickel powder, copper powder, and silver-coated copper, other metal conductive fillers such as gold, silver, aluminum, zinc, iron, silver-coated nickel powder, and one or more mixtures of conductive compounds are applicable to the present invention; one or more mixtures of conductive non-metals are applicable to the present invention, and conductive non-metals such as graphite powder, sintered graphene powder, or carbon black are applicable.
[0153] 3. Under stirring, add the other additives (acrylate rubber, curing agent, accelerator, silane coupling agent, inhibitor) except the metal conductive filler in step 2) to the solution A prepared in step 1) in sequence, wherein the order of addition is acrylate rubber, dicyandiamide, triethylamine accelerator, silane coupling agent KH560, antioxidant 1076, and the stirring rate is 1000 rpm (usually ≥500 rpm);
[0154] 4. After adding the auxiliary raw materials except the metal conductive filler in sequence, continue stirring for 10 minutes to obtain the base glue; then add the metal conductive filler to the base glue under stirring, continue stirring for 30 minutes, stir and mix evenly, and obtain the modified nitrile rubber conductive glue of the present invention;
[0155] 5. Transfer the prepared modified nitrile rubber conductive glue into a rubber barrel, cover it with a lid and seal it with tape, then store it in a low temperature environment of 2-10°C for future use.
[0156] Example 5A: Preparation of conductive adhesive film
[0157] The conductive glue prepared in Example 5 is coated on the release film by a coater, wherein the coater temperature is 100°C (usually 85-160°C); the coating thickness is 60μm (usually 50-70μm); then a drying treatment is performed, wherein the drying tunnel temperature is controlled to be 100°C (usually 80°C~130°C); the solvent is dried to form a film, which is rolled up and placed in a drying room at 35~45°C for curing for 24~48 hours to obtain a conductive adhesive film.
[0158] Test Example 1: Conductive Glue Performance Test
[0159] The conductive glue prepared in Example 1-5 is coated on the central area of the surface of two copper foils, and the two copper foils are aligned and bonded together (to ensure that the glue does not leak out), the surface area and thickness of the two copper foils are the same; the width of the copper foil is 1 cm, and the length is 15 cm; then the two copper foils bonded together are hot-pressed at a temperature of 180° C. and a pressure of 120 kg for 150 seconds, and the conductive glue is cured; the two copper foils are bonded together to obtain a sample to be tested;
[0160] Use a multi-point pen to measure the resistance on the other side of the two copper foils. The results are shown in Table 1.
[0161] Then, the copper foil on one side of the sample to be tested is fixed on the 90° peel strength tester with the clamp of the 90° peel strength tester to test the peel strength of the glue bonding. The test results are shown in Table 1:
[0162] Table 1 Test results of conductive glue performance indicators
[0163] Conductivity / Ω <![CDATA[Peeling strength / kgf / cm 2 > Example 1 0.22 1.7 Example 2 0.19 1.6 Example 3 0.24 1.7 Example 4 0.2 1.5 Example 5 0.24 1.7
[0164] The conductive glue of the present invention has good conductivity, a resistance lower than 0.24Ω, and a resistance value of 0.19-0.24Ω; it has excellent conductivity, reaching the electronic level (less than 1 ohm), and can be used in precision circuits. Compared with other types of conductive glues with a resistance greater than 1 ohm, it has stronger electrical properties and a wider range of applications;
[0165] The peel strength of the product using the glue of the present invention is high, reaching 1.5kgf / cm 2 Above; excellent peel strength performance, significantly higher than the industry standard (≥1kgf / cm 2 ) requirements, suitable for some long-term use and high-demand scenarios, such as: smart displays in cars, urban outdoor electronic displays, etc.
[0166] Test Example 2: Conductive film performance test
[0167] The conductive adhesive film prepared in Examples 1A-5A was attached to the surfaces of two copper foils, and then the two copper foils were aligned and bonded together (ensuring that the adhesive film did not leak out), the surface area and thickness of the two copper foils were the same; the width of the copper foil was 1 cm, and the length was 15 cm; then the two copper foils bonded together were hot-pressed at a temperature of 180° C. and a pressure of 120 kg for 150 seconds, and the conductive adhesive film was cured; the two copper foils were bonded together to obtain a sample to be tested;
[0168] Use a multi-point pen to measure the resistance on the other side of the two copper foils. The results are shown in Table 2.
[0169] Then, the copper foil on one side of the sample to be tested was fixed on a 90° peel strength tester to test the peel strength of the glue (i.e., the copper foil on one side of the sample to be tested was fixed on the 90° peel strength tester with the fixture of the 90° peel strength tester). The test results are shown in Table 2:
[0170] Table 2 Conductive film performance test results
[0171] Conductivity / Ω <![CDATA[Peeling strength / kgf / cm 2 > Example 1A 0.21 ≥2 Example 2A 0.2 ≥2 Example 3A 0.22 ≥2 Example 4A 0.2 ≥2 Example 5A 0.18 ≥2
[0172] According to the test results in Table 1 and Table 2:
[0173] The conductive glue / film of the present invention has good conductivity, and the resistance is less than 0.25 ohms. According to my country's industry standard for conductive adhesives (conductive adhesives) HG / T 5912-2021, the test resistance of the samples prepared by the conductive glue prepared by Examples 1-5 of the present invention is much less than 1 ohm specified in the industry standard. The conductive glue of the present invention has excellent resistance performance, indicating that a chemical reaction occurs between the conductive filler and the matrix glue used in the present invention, and chemical bonds, coordination bonds, etc. are formed between the conductive filler and the matrix glue. In the preparation process of the conductive glue of the present invention, after adding the conductive metal filler, part of the metal is oxidized to produce metal ions and free electrons, which react with the carboxylate on its side chain under the acidic conditions provided by the acrylate resin to form chemical bonds, thereby improving the stability of the product and increasing the intermolecular force; the inhibitor makes most of the added metal fillers passivated and non-reactive, thereby ensuring the activity and conductivity of the metal in the glue.
[0174] The conductive glue or conductive film made by the method of forming chemical bonds in the present invention has significantly improved conductive properties compared to the conductive glue or film prepared by simply physically mixing conductive fillers and base glue. This is mainly reflected in that in practical applications, the dispersion of the conductive fillers is more uniform and more stable, and the conductive properties are also more stable.
[0175] The conductive glue / film of the present invention has excellent peel strength, which is stronger than the bonding performance of most conductive glues and films on the market. The basic standard of glass strength of conductive glue / film in the industry is ≥1kgf / cm 2 The peel strength of the conductive glue / film of the present invention exceeds this standard, and the peel strength is higher than 1.5kgf / cm 2 , it is still applicable in some application scenarios that require higher peel strength.
[0176] During the preparation process of the conductive glue of the present invention, the metal conductive filler reacts chemically with the base glue, and the metal forms a coordination complex bond with the organic acid radical ion, thereby improving the stability and bonding strength of the glue.
[0177] Test Example 3: Weathering Test
[0178] Most of the conductive glues and films on the market have poor aging resistance and weather resistance, and are difficult to pass the conventional high temperature and high humidity double 85 test. In addition, their resistance to organic solvents, acids and alkalis is also not as stable as the internal structure of the product of the present invention, which easily causes a decrease in peeling force, resulting in falling off, loosening, and increased resistance.
[0179] The conductive glue of the present invention overcomes the problem of poor weather resistance. The glue itself is insufficient in strength under high temperature and high humidity or low temperature conditions. Due to differences in curing processes in different usage scenarios, conventional conductive glues will suffer from decreased adhesion and decreased conductivity if they are slightly insufficiently cured. The bonding reaction is equivalent to adding an extra insurance measure, making the product performance more stable.
[0180] The samples prepared in Test Example 2 were placed in a high temperature and high humidity chamber (85°C, relative humidity 85%), and the resistance and peeling force of the samples were continuously tested after 120h, 240h, and 500h. The test method was the same as that in Test Example 2, and the test results are shown in Tables 3-5.
[0181] Table 3 Test results of conductive film performance after being placed in high temperature and high humidity environment for 120 hours
[0182]
[0183]
[0184] Table 4 Test results of conductive film performance after being placed in high temperature and high humidity environment for 240 hours
[0185] Conductivity / Ω <![CDATA[Peeling strength / kgf / cm 2 > Example 1A 0.2 ≥2 Example 2A 0.2 ≥2 Example 3A 0.17 ≥2 Example 4A 0.24 ≥2 Example 5A 0.22 ≥2
[0186] Table 5 Test results of conductive film performance after being placed in high temperature and high humidity environment for 500 hours
[0187] Conductivity / Ω <![CDATA[Peeling strength / kgf / cm 2 > Example 1A 0.22 ≥2 Example 2A 0.25 ≥2 Example 3A 0.2 ≥2 Example 4A 0.22 ≥2 Example 5A 0.2 ≥2
[0188] From the test results in Table 3-5, we can see that:
[0189] The conductive glue / film of the present invention has strong weather resistance and high product stability, good conductivity in a high temperature and high humidity environment, and the resistance value is still lower than 0.25Ω after being placed for 500 hours, and the conductive performance is not reduced; the peel strength is high, the bonding performance is not reduced, and the peel strength is higher than 2kgf / cm 2 ; It will not fall off or loosen in high temperature and high humidity environments, which enhances the aging resistance and weather resistance of the glue / film, increases the application range of the product, and extends the service life of the product.
[0190] The above description is only a preferred embodiment of the present invention and does not limit the technical scope of the present invention. Therefore, any slight modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention are still within the scope of the technical solution of the present invention.
Claims
1. A method for preparing a modified nitrile rubber-based conductive glue, characterized in that: The steps include the following steps in order: 1) stirring and mixing the raw materials of nitrile rubber, ketone solvent, bisphenol A epoxy resin, phenolic resin, polyimide and / or bismaleimide to obtain a nitrile rubber solution, i.e., obtaining solution A; 2) Under stirring, adding functional additives to solution A in sequence, stirring and mixing evenly to obtain a matrix glue; 3) Adding metal conductive filler into the base glue under stirring to obtain nitrile rubber-based conductive glue.
2. The preparation method according to claim 1, characterized in that: The weight proportion of the raw materials nitrile rubber, ketone solvent, bisphenol A epoxy resin, phenolic resin, polyimide and / or bismaleimide in step 1) is:
3. The preparation method according to claim 1 or 2, characterized in that: The solvent in step 1) is one or more of toluene, acetone, butanone, cyclohexanone, ethyl acetate, and butyl acetate.
4. The preparation method according to claim 1 or 2, characterized in that: The functional additives in step 2) are one or more of acrylic rubber, curing agent, accelerator, coupling agent and inhibitor.
5. The preparation method according to claim 4, characterized in that: The acid value of the acrylic rubber is greater than 50 (KOH) / (mg / g), preferably 50-60 (KOH) / (mg / g); and the molecular weight is greater than 1000 Da, preferably 1000-1500 Da.
6. The preparation method according to claim 1 or 2, characterized in that: The weight ratio of the added metal conductive filler in step 3) is 20-35.
7. The preparation method according to claim 1 or 2, characterized in that: The metal conductive filler in step 3) is one or more of nickel powder, copper powder, silver powder, gold powder, silver-coated copper powder, gold-coated nickel powder, nickel-coated glass microspheres, copper-coated glass microspheres, silver-coated glass microspheres, and graphite powder.
8. A modified nitrile rubber-based conductive glue, characterized in that: Prepared according to the method as described in any one of claims 1 to 7.
9. A method for preparing a modified nitrile rubber-based conductive film, characterized in that: The steps include: A) stirring and mixing nitrile rubber, ketone solvent, bisphenol A type epoxy resin, phenolic resin, polyimide and / or bismaleimide to obtain a nitrile rubber solution, i.e., obtaining solution A; B) adding functional additives to solution A in sequence under stirring, stirring and mixing evenly to obtain a matrix glue; C) adding a metal conductive filler to the base glue under stirring to obtain a nitrile rubber-based conductive glue; D) The conductive glue is coated on the release film, followed by drying, drying the solvent to form a film, and then curing to obtain a conductive adhesive film.
10. A modified nitrile rubber-based conductive film, characterized in that: Prepared according to the method as claimed in claim 9.