Yellowing-resistant adhesive for photovoltaic module and application of yellowing-resistant adhesive in assembly of photovoltaic module
By using aliphatic polyester resins containing adamantane structures to improve the yellowing resistance and mechanical properties of UV-curable adhesives, the problems of insufficient yellowing resistance and small molecule migration of existing adhesives in photovoltaic modules are solved, and high-reliability photovoltaic module encapsulation is achieved.
Patent Information
- Application Number
- CN202411011892.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-08
AI Technical Summary
Existing UV-curable adhesives have insufficient resistance to yellowing and small molecule migration in low-temperature encapsulation processes, which cannot meet the high reliability requirements of HJT or Topcon photovoltaic cells.
Using aliphatic polyester resin containing adamantane structure as the main material, the adhesive’s resistance to yellowing and mechanical properties are improved by introducing a molecular structure that does not produce chromophores and combining it with self-crosslinking of siloxane groups.
The adhesive for photovoltaic modules exhibits excellent resistance to yellowing, low molecular migration, and high strength, meeting the design requirements of photovoltaic modules.
Smart Images

Figure BDA0004964619800000021 
Figure BDA0004964619800000111 
Figure BDA0004964619800000121
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of adhesives, and in particular to a yellowing-resistant adhesive for photovoltaic modules and application thereof in photovoltaic module assembly. Background Art
[0002] With the continuous development of solar photovoltaic technology, new battery assembly processes and technologies emerge in an endless stream. The original PERC (Passivated Emitter and Rear Cell) process is gradually being replaced by HJT (Heterojunction Technology, amorphous silicon thin film) heterojunction battery process or Topcon (Tunnel Oxide Passivating Contacts) tunnel oxide passivating contact battery process.
[0003] Due to the low-temperature process characteristics of HJT or Topcon photovoltaic cells, the subsequent high-temperature packaging process used by traditional crystalline silicon cells cannot be adopted, and traditional soldering (soldering) is increasingly unable to meet the requirements of the cell assembly process in terms of efficiency and adhesion. Therefore, it is necessary to develop a suitable low-temperature packaging process.
[0004] Currently, in the low-temperature packaging process, UV light-curing adhesives are used to replace part of the welding to achieve structural assembly. Although this method has the advantages of simple operation, low energy consumption, and low material cost, the UV light-curing adhesives used in the existing research process have their own limitations. For example, conventional UV light-curing adhesives have obvious limitations in the application scenarios of yellowing resistance and small molecule migration, and UV light-curing adhesives cannot meet the design requirements of photovoltaic modules in terms of performance such as strength after curing. Summary of the invention
[0005] Based on the technical problems existing in the background technology, the present invention proposes a yellowing-resistant adhesive for photovoltaic modules and its application in photovoltaic module assembly. The adhesive has excellent resistance to UV yellowing and low molecular weight migration, as well as good strength and high-humidity aging resistance, and can be cured at room temperature and used at high temperatures, thereby meeting the high-reliability photovoltaic application requirements.
[0006] The present invention provides a yellowing-resistant adhesive for photovoltaic modules, wherein the raw materials include, by weight: 50 parts of aliphatic polyester resin A, 10-30 parts of aliphatic polyester resin B, 50-200 parts of acrylate monomers, 1-5 parts of curing agent, and 0.1-1 part of accelerator;
[0007] The aliphatic polyester resin A is an unsaturated polyester resin including a diol containing an adamantane structure as shown in the structural formula I; the aliphatic polyester resin B is a saturated polyester resin including a dibasic acid anhydride containing an adamantane structure as shown in the structural formula II;
[0008]
[0009] Wherein, n is an integer greater than 1, and R is a C1-C4 alkyl group.
[0010] For those skilled in the art, UV-curing adhesives usually use polyurethane acrylate as the main ingredient. Since the carbamate groups contained in its molecular chain will break bonds under the irradiation of ultraviolet light, the broken bonds will produce colored groups such as imide, causing its absorption wavelength to shift to the long-wave direction, macroscopically causing the material to color or make its color turn yellow and deepen; considering that the polyurethane acrylate main ingredient used in UV-curing adhesives has an inherent defect that cannot improve its yellowing resistance, the present invention uses aliphatic polyester resin as the main ingredient. On the one hand, there are no chromogenic groups such as carbamate in its molecular chain structure, so the yellowing of the adhesive can be fundamentally avoided; on the other hand, the aliphatic polyester resin also has structural groups such as adamantane, and adamantane has good structural regularity and rigidity, which can not only further improve the yellowing resistance of the resin, but also improve the mechanical properties and moisture-heat aging resistance of the resin.
[0011] Preferably, the adamantane structure-containing diol represented by structural formula I is formed by condensing 1,3-adamantanedicarboxylic acid chloride with a linear diol.
[0012] Preferably, the dibasic acid anhydride containing adamantane structure shown in structural formula II is formed by coupling 1,3,5-adamantanetriol with alkoxysilane succinic anhydride.
[0013] In the present invention, after the diol containing adamantane structure shown in structural formula I and the dibasic acid anhydride containing adamantane structure shown in structural formula II are introduced into the polyester resin as monomers, on the one hand, their larger three-dimensional structure volume can achieve high free volume, thereby improving the light transmittance and yellowing resistance of the resin; on the other hand, the dibasic acid anhydride containing adamantane structure shown in structural formula II is grafted into the main chain of the polyester resin as a side chain structure. Since the adamantane structure is modified by the group of the silane coupling agent, the siloxy groups contained therein can also self-crosslink with the hydroxyl groups in the polyester resin, thereby further improving the mechanical strength and moisture-heat aging resistance of the obtained adhesive, while also reducing the curing temperature.
[0014] Preferably, the aliphatic polyester resin A is formed by polycondensing an aliphatic unsaturated dibasic acid or anhydride, an aliphatic saturated dibasic acid or anhydride, an aliphatic polyol, and an adamantane structure-containing diol as shown in structural formula I;
[0015] Preferably, the molar ratio of the aliphatic unsaturated dibasic acid or anhydride, the aliphatic saturated dibasic acid or anhydride, the aliphatic polyol and the adamantane structure-containing diol represented by structural formula I is 1:0.2-0.4:0.7-0.9:0.4-0.6.
[0016] Preferably, the aliphatic polyester resin B is formed by polycondensing an aliphatic saturated dibasic acid or anhydride, a dibasic acid anhydride containing an adamantane structure as shown in structural formula II, and an aliphatic polyol;
[0017] Preferably, the molar ratio of the aliphatic saturated dibasic acid or anhydride, the dibasic acid anhydride containing the adamantane structure shown in structural formula II and the aliphatic polyol is 1:0.1-0.3:0.9-1.1.
[0018] Preferably, the aliphatic unsaturated dibasic acid or anhydride is at least one of maleic anhydride, fumaric acid, itaconic acid or itaconic anhydride;
[0019] Preferably, the aliphatic saturated dibasic acid or anhydride is at least one of 1,4-succinic acid, 1,6-hexanodioic acid, succinic anhydride, adipic anhydride, 1,4-cyclohexanediacid, 1,2-cyclohexanediacid or 1,2-cyclohexanedicarboxylic anhydride;
[0020] Preferably, the aliphatic polyol is at least one of 1,3-propylene glycol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, neopentyl glycol, diethylene glycol, dipropylene glycol, 1,10-decanediol, 1,4-cyclohexanedimethanol or a hydroxyl-terminated polyglycol.
[0021] Preferably, the acrylic acid ester monomer is at least one of methyl crotonate, tripropylene glycol diacrylate, 1,6-hexanediol diacrylate, isobornyl acrylate, hydroxyethyl acrylate, diethylene glycol diacrylate or isobutyl acrylate.
[0022] Preferably, the curing agent is at least one of benzoyl peroxide, dicumyl peroxide, tert-butyl perbenzoate, methyl ethyl ketone peroxide or cyclohexanone peroxide.
[0023] Preferably, the promoter is at least one of cobalt isooctanoate, potassium isooctanoate, copper isooctanoate or copper naphthenate.
[0024] The present invention also provides an application of the yellowing-resistant adhesive in the assembly of photovoltaic modules.
[0025] Compared with the prior art, the present invention has the following beneficial effects:
[0026] (1) The present invention improves the yellowing resistance of the adhesive by introducing an aliphatic polyester resin that does not generate a chromophore group from the polymer structure, and has a more durable and better yellowing resistance than the conventional method of adding an ultraviolet absorber to improve the yellowing resistance of the adhesive.
[0027] (2) The present invention selects a diol containing adamantane structure and a dibasic acid anhydride containing adamantane structure to synthesize aliphatic polyester resin and uses it for adhesive, thereby obtaining an adhesive for photovoltaic modules having both excellent yellowing resistance and mechanical strength properties.
[0028] (3) The anti-yellowing adhesive for photovoltaic modules of the present invention achieves a very excellent overall effect, and can fully meet the design requirements of photovoltaic modules in terms of adhesion, strength, anti-yellowing and other properties. DETAILED DESCRIPTION
[0029] The technical solutions of the present invention are described in detail below through specific embodiments. However, it should be clearly stated that these embodiments are for illustration only and are not to be construed as limiting the scope of the present invention.
[0030] Example 1
[0031] A yellowing-resistant adhesive for photovoltaic modules, the raw materials of which include, by weight: 50 parts of aliphatic polyester resin A, 20 parts of aliphatic polyester resin B, 100 parts of acrylate monomers, 2 parts of curing agent, and 0.5 parts of accelerator;
[0032] The preparation method of the above-mentioned yellowing-resistant adhesive for photovoltaic modules is as follows:
[0033] (1) Preparation of aliphatic polyester resin A: under nitrogen protection, maleic anhydride, 1,4-butanedioic acid, 1,6-hexanediol and a diol containing adamantane structure shown in structural formula I are added to a reaction kettle in a molar ratio of 1:0.3:0.8:0.5, stirred and mixed evenly, slowly heated to 160° C. and kept warm for 1 hour, tetrabutyl titanate of 0.1 wt % of the total weight of the reactants is added, slowly heated to 200° C. and kept warm for 2 hours, cooled to 180° C., evacuated the reaction kettle to a vacuum degree of 0.6 MPa, kept warm for 2 hours, and a polymerization inhibitor hydroquinone of 0.01 wt % of the total weight of the reactants is added, and the reaction is completed to obtain aliphatic polyester resin A;
[0034] The adamantane diol shown in the structural formula I is prepared by referring to the following method: 1,3-adamantanedicarboxylic acid chloride is added to an ethylene glycol solvent, the temperature is raised to 120° C., and the mixture is stirred for reaction for 6 hours. The ethylene glycol is removed by vacuum distillation, and the adamantane diol shown in the structural formula I is obtained.
[0035] (2) Preparation of aliphatic polyester resin B: under nitrogen protection, 1,4-butanediol, dibasic acid anhydride containing adamantane structure shown in structural formula II and 1,6-hexanediol were added to a reaction kettle in a molar ratio of 1:0.2:1, stirred and mixed evenly, slowly heated to 160° C. and kept warm for 1 hour, then slowly heated to 200° C. and kept warm for 2 hours, cooled to 160° C., evacuated the reaction kettle to a vacuum degree of 0.6 MPa, kept warm for 1 hour, and added 0.01 wt% of the total weight of the reactants as a polymerization inhibitor hydroquinone, and the reaction was completed to obtain aliphatic polyester resin B;
[0036] The dibasic acid anhydride containing adamantane structure shown in structural formula II is prepared by referring to the following method: 1,3,5-adamantantriol and (3-triethoxysilyl)propylsuccinic anhydride are added to ethanol at a molar ratio of 1:1, the mixture is heated to 80° C. and stirred for reaction for 24 hours, and the ethanol is removed by vacuum distillation to obtain the dibasic acid anhydride containing adamantane structure shown in structural formula II;
[0037] (3) Preparation of a yellowing-resistant adhesive for photovoltaic modules: 50 parts by weight of the aliphatic polyester resin A and 20 parts by weight of the aliphatic polyester resin B are added into a vacuum mixer, heated to 80° C., 50 parts of an acrylate monomer (methyl crotonate) and 50 parts of an acrylate monomer (isobornyl acrylate) are added, and the mixture is stirred and mixed evenly. The mixture is cooled to room temperature, and 2 parts of a curing agent (benzoyl peroxide) and 0.5 parts of an accelerator (cobalt isooctanoate) are added. The mixture is stirred and mixed under vacuum for 0.5 h to obtain the yellowing-resistant adhesive for photovoltaic modules.
[0038] Example 2
[0039] A yellowing-resistant adhesive for photovoltaic modules, the raw materials of which include, by weight: 50 parts of aliphatic polyester resin A, 30 parts of aliphatic polyester resin B, 50 parts of acrylate monomers, 1 part of curing agent, and 1 part of accelerator;
[0040] The preparation method of the above-mentioned yellowing-resistant adhesive for photovoltaic modules is as follows:
[0041] (1) Preparation of aliphatic polyester resin A: The method described in step (1) of Example 1 is referred to, except that itaconic acid, 1,4-cyclohexane diacid, 1,3-propylene glycol and a diol containing adamantane structure represented by structural formula I are added to a reaction kettle in a molar ratio of 1:0.2:0.9:0.4;
[0042] (2) Preparation of aliphatic polyester resin B: The method described in step (2) of Example 1 is referred to, except that 1,4-cyclohexane diacid, a dibasic acid anhydride containing adamantane structure represented by structural formula II and 1,3-propylene glycol are added to a reaction kettle in a molar ratio of 1:0.1:1.1;
[0043] (3) Preparation of a yellowing-resistant adhesive for photovoltaic modules: 50 parts of the above-mentioned aliphatic polyester resin A and 30 parts of the aliphatic polyester resin B are added into a vacuum mixer by weight, and the temperature is raised to 80° C., and 30 parts of an acrylate monomer (diethylene glycol diacrylate) and 20 parts of an acrylate monomer (isobornyl acrylate) are added. After stirring and mixing evenly, the mixture is cooled to room temperature, and 1 part of a curing agent (benzoyl peroxide) and 1 part of an accelerator (cobalt isooctanoate) are added. After stirring and mixing under vacuum for 0.5 h, the yellowing-resistant adhesive for photovoltaic modules is obtained.
[0044] Example 3
[0045] A yellowing-resistant adhesive for photovoltaic modules, the raw materials of which include, by weight: 50 parts of aliphatic polyester resin A, 10 parts of aliphatic polyester resin B, 200 parts of acrylate monomers, 5 parts of curing agent, and 0.1 parts of accelerator;
[0046] The preparation method of the above-mentioned yellowing-resistant adhesive for photovoltaic modules is as follows:
[0047] (1) Preparation of aliphatic polyester resin A: The method described in step (1) of Example 1 is referred to, except that maleic anhydride, 1,4-cyclohexane diacid, neopentyl glycol and adamantane structure-containing diol represented by structural formula I are added to a reaction kettle in a molar ratio of 1:0.4:0.7:0.6;
[0048] (2) Preparation of aliphatic polyester resin B: The method described in step (2) of Example 1 is referred to, except that 1,4-cyclohexane diacid, a dibasic acid anhydride containing adamantane structure represented by structural formula II and neopentyl glycol are added to the reaction kettle in a molar ratio of 1:0.3:0.9;
[0049] (3) Preparation of yellowing-resistant adhesive for photovoltaic modules: 50 parts by weight of the aliphatic polyester resin A and 10 parts by weight of the aliphatic polyester resin B are added into a vacuum mixer, heated to 80° C., 50 parts of acrylate monomer (methyl crotonate) and 150 parts of acrylate monomer (isobornyl acrylate) are added, and the mixture is stirred and mixed evenly. The mixture is cooled to room temperature, and 5 parts of curing agent (benzoyl peroxide) and 0.1 parts of accelerator (cobalt isooctanoate) are added. The mixture is stirred and mixed under vacuum for 0.5 h to obtain the yellowing-resistant adhesive for photovoltaic modules.
[0050] Comparative Example 1
[0051] A yellowing-resistant adhesive for photovoltaic modules, the raw materials of which include, by weight: 50 parts of aliphatic polyester resin A', 20 parts of aliphatic polyester resin B', 100 parts of acrylate monomers, 2 parts of curing agent, and 0.5 parts of accelerator;
[0052] The preparation method of the above-mentioned yellowing-resistant adhesive for photovoltaic modules is as follows:
[0053] (1) Preparation of aliphatic polyester resin A': under nitrogen protection, maleic anhydride, 1,4-butanedioic acid and 1,6-hexanediol were added to a reaction kettle in a molar ratio of 1:0.3:1.3, stirred and mixed evenly, slowly heated to 160° C. and kept warm for 1 hour, added tetrabutyl titanate in an amount of 0.1 wt % of the total weight of the reactants, slowly heated to 200° C. and kept warm for 2 hours, cooled to 180° C., evacuated the reaction kettle to a vacuum degree of 0.6 MPa, kept warm for 2 hours, added a polymerization inhibitor hydroquinone in an amount of 0.01 wt % of the total weight of the reactants, and the reaction was completed to obtain aliphatic polyester resin A';
[0054] (2) Preparation of aliphatic polyester resin B': under nitrogen protection, 1,4-butanediol and 1,6-hexanediol were added to a reaction kettle in a molar ratio of 1.2:1 and stirred to mix evenly, and the temperature was slowly raised to 160° C. and kept warm for 1 hour, and then slowly raised to 200° C. and kept warm for 2 hours, and then cooled to 160° C., the reaction kettle was evacuated to a vacuum degree of 0.6 MPa, and kept warm for 1 hour, and a polymerization inhibitor hydroquinone was added in an amount of 0.01 wt% of the total mass of the reactants, and the reaction was completed to obtain aliphatic polyester resin B';
[0055] (3) Preparation of yellowing-resistant adhesive for photovoltaic modules: 50 parts of the above-mentioned aliphatic polyester resin A' and 20 parts of the aliphatic polyester resin B' are added into a vacuum mixer by weight, and the temperature is raised to 80°C. 50 parts of acrylic acid ester monomer (methyl crotonate) and 50 parts of acrylic acid ester monomer (isobornyl acrylate) are added. After stirring and mixing evenly, the mixture is cooled to room temperature, 2 parts of curing agent (benzoyl peroxide) and 0.5 parts of accelerator (cobalt isooctanoate) are added, and the mixture is stirred and mixed under vacuum for 0.5 hours to obtain the yellowing-resistant adhesive for photovoltaic modules.
[0056] Comparative Example 2
[0057] A yellowing-resistant adhesive for photovoltaic modules, the raw materials of which include, by weight: 50 parts of aliphatic polyester resin A, 20 parts of aliphatic polyester resin B', 100 parts of acrylate monomers, 2 parts of curing agent, and 0.5 parts of accelerator;
[0058] The preparation method of the above-mentioned yellowing-resistant adhesive for photovoltaic modules is as follows:
[0059] (1) Preparation of aliphatic polyester resin A: under nitrogen protection, maleic anhydride, 1,4-butanedioic acid, 1,6-hexanediol and a diol containing adamantane structure shown in structural formula I are added to a reaction kettle in a molar ratio of 1:0.3:0.8:0.5, stirred and mixed evenly, slowly heated to 160° C. and kept warm for 1 hour, tetrabutyl titanate of 0.1 wt % of the total weight of the reactants is added, slowly heated to 200° C. and kept warm for 2 hours, cooled to 180° C., evacuated the reaction kettle to a vacuum degree of 0.6 MPa, kept warm for 2 hours, and a polymerization inhibitor hydroquinone of 0.01 wt % of the total weight of the reactants is added, and the reaction is completed to obtain aliphatic polyester resin A;
[0060] The adamantane diol shown in the structural formula I is prepared by referring to the following method: 1,3-adamantanedicarboxylic acid chloride is added to an ethylene glycol solvent, the temperature is raised to 120° C., and the mixture is stirred for reaction for 6 hours. The ethylene glycol is removed by vacuum distillation, and the adamantane diol shown in the structural formula I is obtained.
[0061] (2) Preparation of aliphatic polyester resin B': under nitrogen protection, 1,4-butanediol and 1,6-hexanediol were added to a reaction kettle in a molar ratio of 1.2:1 and stirred to mix evenly, and the temperature was slowly raised to 160° C. and kept warm for 1 hour, and then slowly raised to 200° C. and kept warm for 2 hours, and then cooled to 160° C., the reaction kettle was evacuated to a vacuum degree of 0.6 MPa, and kept warm for 1 hour, and a polymerization inhibitor hydroquinone was added in an amount of 0.01 wt% of the total mass of the reactants, and the reaction was completed to obtain aliphatic polyester resin B';
[0062] (3) Preparation of yellowing-resistant adhesive for photovoltaic modules: 50 parts by weight of the aliphatic polyester resin A and 20 parts by weight of the aliphatic polyester resin B' are added into a vacuum mixer, heated to 80°C, 50 parts of acrylate monomer (methyl crotonate) and 50 parts of acrylate monomer (isobornyl acrylate) are added, and the mixture is stirred and mixed evenly. The mixture is cooled to room temperature, 2 parts of curing agent (benzoyl peroxide) and 0.5 parts of accelerator (cobalt isooctanoate) are added, and the mixture is stirred and mixed under vacuum for 0.5 h to obtain the yellowing-resistant adhesive for photovoltaic modules.
[0063] Comparative Example 3
[0064] A yellowing-resistant adhesive for photovoltaic modules, the raw materials of which include, by weight: 50 parts of aliphatic polyester resin A', 20 parts of aliphatic polyester resin B, 100 parts of acrylate monomers, 2 parts of curing agent, and 0.5 parts of accelerator;
[0065] The preparation method of the above-mentioned yellowing-resistant adhesive for photovoltaic modules is as follows:
[0066] (1) Preparation of aliphatic polyester resin A': under nitrogen protection, maleic anhydride, 1,4-butanedioic acid and 1,6-hexanediol were added to a reaction kettle in a molar ratio of 1:0.3:1.3, stirred and mixed evenly, slowly heated to 160° C. and kept warm for 1 hour, added tetrabutyl titanate in an amount of 0.1 wt % of the total weight of the reactants, slowly heated to 200° C. and kept warm for 2 hours, cooled to 180° C., evacuated the reaction kettle to a vacuum degree of 0.6 MPa, kept warm for 2 hours, added a polymerization inhibitor hydroquinone in an amount of 0.01 wt % of the total weight of the reactants, and the reaction was completed to obtain aliphatic polyester resin A';
[0067] (2) Preparation of aliphatic polyester resin B: under nitrogen protection, 1,4-butanediol, dibasic acid anhydride containing adamantane structure shown in structural formula II and 1,6-hexanediol were added to a reaction kettle in a molar ratio of 1:0.2:1, stirred and mixed evenly, slowly heated to 160° C. and kept warm for 1 hour, then slowly heated to 200° C. and kept warm for 2 hours, cooled to 160° C., evacuated the reaction kettle to a vacuum degree of 0.6 MPa, kept warm for 1 hour, and added 0.01 wt% of the total weight of the reactants as a polymerization inhibitor hydroquinone, and the reaction was completed to obtain aliphatic polyester resin B;
[0068] The dibasic acid anhydride containing adamantane structure shown in structural formula II is prepared by referring to the following method: 1,3,5-adamantantriol and (3-triethoxysilyl)propylsuccinic anhydride are added to ethanol at a molar ratio of 1:1, the mixture is heated to 80° C. and stirred for reaction for 24 hours, and the ethanol is removed by vacuum distillation to obtain the dibasic acid anhydride containing adamantane structure shown in structural formula II;
[0069] (3) Preparation of yellowing-resistant adhesive for photovoltaic modules: 50 parts of the above-mentioned aliphatic polyester resin A' and 20 parts of aliphatic polyester resin B are added into a vacuum mixer by weight, and the mixture is heated to 80°C, and 50 parts of acrylate monomer (methyl crotonate) and 50 parts of acrylate monomer (isobornyl acrylate) are added. After stirring and mixing evenly, the mixture is cooled to room temperature, and 2 parts of curing agent (benzoyl peroxide) and 0.5 parts of accelerator (cobalt isooctanoate) are added. After stirring and mixing under vacuum for 0.5 h, the yellowing-resistant adhesive for photovoltaic modules is obtained.
[0070] Performance Test:
[0071] After the yellowing-resistant adhesives obtained in the above examples and comparative examples were cured at high temperature, the following performance tests were performed. The results are shown in Table 1 below.
[0072] The tensile strength is measured according to standard GB / T528-2009;
[0073] The light transmittance is measured according to the standard GB / T2410-2008, specifically the light transmittance of a 0.45mm thick film at 400-1100nm;
[0074] The bonding strength is measured according to the standard ASTM D1002, specifically, a 5mm×5mm bonding area is marked on a 2mm thick glass sheet, and the yellowing-resistant adhesive is evenly coated thereon, with a film thickness of 0.2mm, and then laminated with a 2mm thick stainless steel sheet, and hot-pressed according to a lamination process of 145°C, 0.07Mpa, and 16min, and fully cured at high temperature (180°C, 5min) to obtain a test sample, and the shear strength is measured at a peeling speed of 50mm / min;
[0075] The moisture and heat resistance performance is to place the above test samples in a high temperature and high humidity oven at 85°C and 85% relative humidity for 1000 hours, and then measure the shear strength at a peeling speed of 50mm / min;
[0076] Yellowing resistance is measured according to ASTM E313-2010 standard. Specifically, the above test samples are placed in a UV aging test chamber and irradiated with UV radiation of 150kWh / m 2 After sampling, the samples were tested for yellowness index before and after the experiment, and the difference in yellowness index before and after the UV accelerated aging test was taken as the yellowing index ΔYI.
[0077] Table 1 Performance test results of the yellowing-resistant adhesives described in Examples and Comparative Examples
[0078]
[0079]
[0080] It can be seen from the above table that the yellowing-resistant adhesive of the present invention has excellent mechanical and yellowing-resistant properties.
[0081] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A yellowing resistant adhesive for photovoltaic modules, It is characterized in that The raw materials include, by weight: 50 parts of aliphatic polyester resin A, 10-30 parts of aliphatic polyester resin B, 50-200 parts of acrylate monomers, 1-5 parts of curing agent, and 0.1-1 part of accelerator; The aliphatic polyester resin A is an unsaturated polyester resin including a diol containing an adamantane structure as shown in the structural formula I; the aliphatic polyester resin B is a saturated polyester resin including a dibasic acid anhydride containing an adamantane structure as shown in the structural formula II; Wherein, n is an integer greater than 1, and R is a C1-C4 alkyl group.
2. The yellowing-resistant adhesive for photovoltaic modules according to claim 1, It is characterized in that The adamantane structure-containing diol shown in structural formula I is formed by condensing 1,3-adamantanedicarboxylic acid chloride with a linear diol.
3. The highly yellowing-resistant adhesive for photovoltaic modules according to claim 1 or 2, It is characterized in that The dibasic acid anhydride containing adamantane structure shown in structural formula II is formed by coupling 1,3,5-adamantanetriol with alkoxysilane succinic anhydride.
4. The yellowing-resistant adhesive for photovoltaic modules according to any one of claims 1 to 3, It is characterized in that The aliphatic polyester resin A is formed by polycondensing an aliphatic unsaturated dibasic acid or anhydride, an aliphatic saturated dibasic acid or anhydride, an aliphatic polyol, and an adamantane structure-containing diol as shown in the structural formula I; Preferably, the molar ratio of the aliphatic unsaturated dibasic acid or anhydride, the aliphatic saturated dibasic acid or anhydride, the aliphatic polyol and the adamantane structure-containing diol represented by structural formula I is 1:0.2-0.4:0.7-0.9:0.4-0.
6.
5. The yellowing-resistant adhesive for photovoltaic modules according to any one of claims 1 to 4, It is characterized in that The aliphatic polyester resin B is formed by polycondensing an aliphatic saturated dibasic acid or anhydride, a dibasic acid anhydride containing an adamantane structure as shown in the structural formula II, and an aliphatic polyol; Preferably, the molar ratio of the aliphatic saturated dibasic acid or anhydride, the dibasic acid anhydride containing the adamantane structure shown in structural formula II and the aliphatic polyol is 1:0.1-0.3:0.9-1.
1.
6. The yellowing-resistant adhesive for photovoltaic modules according to claim 4 or 5, It is characterized in that The aliphatic unsaturated dibasic acid or anhydride is at least one of maleic anhydride, fumaric acid, itaconic acid or itaconic anhydride; Preferably, the aliphatic saturated dibasic acid or anhydride is at least one of 1,4-succinic acid, 1,6-hexanodioic acid, succinic anhydride, adipic anhydride, 1,4-cyclohexanediacid, 1,2-cyclohexanediacid or 1,2-cyclohexanedicarboxylic anhydride; Preferably, the aliphatic polyol is at least one of 1,3-propylene glycol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, neopentyl glycol, diethylene glycol, dipropylene glycol, 1,10-decanediol, 1,4-cyclohexanedimethanol or a hydroxyl-terminated polyglycol.
7. The yellowing-resistant adhesive for photovoltaic modules according to any one of claims 1 to 6, It is characterized in that The acrylic acid ester monomer is at least one of methyl crotonate, tripropylene glycol diacrylate, 1,6-hexanediol diacrylate, isobornyl acrylate, hydroxyethyl acrylate, diethylene glycol diacrylate or isobutyl acrylate.
8. The anti-yellowing adhesive for photovoltaic modules according to any one of claims 1 to 7, It is characterized in that The curing agent is at least one of benzoyl peroxide, dicumyl peroxide, tert-butyl perbenzoate, methyl ethyl ketone peroxide or cyclohexanone peroxide.
9. The yellowing-resistant adhesive for photovoltaic modules according to any one of claims 1 to 8, It is characterized in that The promoter is at least one of cobalt isooctanoate, potassium isooctanoate, copper isooctanoate or copper naphthenate.
10. Use of the yellowing-resistant adhesive according to any one of claims 1 to 9 in the assembly of photovoltaic modules.
Citation Information
Cited By
Single-component high-strength fast-curing adhesive and preparation method thereof
CN121343503A