LED curing battery protection glue and preparation method thereof

By combining aliphatic polyurethane acrylate and epoxy-modified acrylate, along with specific adhesion promoters and fillers, an LED-curable battery protective adhesive was prepared. This adhesive solved the problems of insufficient electrolyte resistance and adhesion performance in lithium batteries, achieving improved corrosion resistance and adhesion performance at high temperatures, and also possessing environmentally friendly and efficient light-curing characteristics.

CN118909585APending Publication Date: 2024-11-08SHANGHAI SATO MATERIAL SCI CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410988409.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Traditional adhesive tapes used in lithium batteries suffer from poor resistance to electrolyte corrosion and decreased adhesion at high temperatures. Existing technologies struggle to simultaneously improve both electrolyte resistance and adhesion.

Method used

A battery protective adhesive was prepared by combining aliphatic polyurethane acrylate and epoxy-modified acrylate, with γ-(methacryloyloxy)propyltrimethoxysilane and phosphate acrylate as adhesion promoters, and using fumed silica, via LED light curing.

Benefits of technology

It improves the electrolyte resistance and adhesion of battery protective adhesive, extends the corrosion resistance time in high-temperature electrolytes, improves storage stability, and has the advantages of energy-saving and environmentally friendly photocuring.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004958159740000041
    Figure BDA0004958159740000041
  • Figure BDA0004958159740000051
    Figure BDA0004958159740000051
  • Figure BDA0004958159740000061
    Figure BDA0004958159740000061
Patent Text Reader

Abstract

The LED curing battery protection glue is prepared from the following raw materials in parts by weight: 40 to 65 parts of aliphatic polyurethane acrylate, 10 to 30 parts of epoxy modified acrylate, 20 to 55 parts of reactive diluent, 3 to 8 parts of initiator, 1 to 5 parts of adhesion promoter and 1 to 5 parts of filler. The composition of the aliphatic polyurethane acrylate and the epoxy modified acrylate is adopted, so that the electrolyte resistance can be optimized, and the corrosion-resistant time in a high-temperature electrolyte can be prolonged. The anti-rust oil can replace the traditional anti-rust oil used for the laser welding hole of the battery, and has the advantages of energy conservation, environmental protection and high efficiency by using 395nm LED light curing; and meanwhile, the properties of salt mist resistance, electrolyte resistance, super-strong adhesive force and the like of the traditional anti-rust oil can be achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to an LED-cured battery protective adhesive and a preparation method thereof, and relates to C09J, and in particular to the field of adhesives. Background Art

[0002] With the rapid development of new energy technologies, mobile phones, tablets and other electronic products are widely used in people's lives. At the same time, higher requirements are put forward for new energy batteries, such as extending battery life, improving fast charging performance, and improving safety of use. In order to ensure the safety of lithium batteries, tape products are used on battery chips, electrodes, and diaphragm fixation. The tape used for lithium batteries needs to have good electrolyte resistance. However, traditional tapes are not resistant to electrolyte corrosion when used in batteries, and there is a heating problem when the battery is used. It is more susceptible to electrolyte corrosion under heating conditions, and the bonding performance is reduced. Therefore, it is crucial to develop a battery protective adhesive that is resistant to high-temperature electrolytes and improve the bonding performance.

[0003] Chinese invention patent CN202210319661.5 discloses a glue for battery protective film tape and its preparation method. The double bond structure is introduced into the glue by the condensation reaction of the hydroxyl functional group of the hydroxyl acrylate monomer and the isocyanate group of the isocyanate monomer. The number average molecular weight distribution is stable and controllable. The formed adhesive film has an appropriate peeling force and is not prone to residual glue, but the electrolyte resistance is poor. Chinese invention patent CN202221558033.4 discloses an electrolyte-resistant tape for lithium battery cells. By designing a four-layer main structure, the comprehensive performance of the tape, such as electrolyte resistance, peeling force, and temperature resistance, can be significantly improved, which provides a guarantee for its safe use inside the battery cell, but the corrosion resistance to electrolytes at high temperatures is poor. Summary of the invention

[0004] In order to improve the electrolyte resistance and salt spray resistance of the battery protective glue, and at the same time improve the bonding adhesion of the battery protective glue, the first aspect of the present invention provides an LED-cured battery protective glue, and the preparation raw materials include, by weight: 40-65 parts of aliphatic polyurethane acrylate, 10-30 parts of epoxy-modified acrylate, 20-55 parts of active diluent, 3-8 parts of initiator, 1-5 parts of adhesion promoter, and 1-5 parts of filler.

[0005] As a preferred embodiment, the raw materials for preparation include, by weight: 40-60 parts of aliphatic polyurethane acrylate, 15-20 parts of epoxy modified acrylate, 30-40 parts of reactive diluent, 4-7 parts of initiator, 2-4 parts of adhesion promoter, and 2-4 parts of filler.

[0006] As a preferred embodiment, the aliphatic polyurethane acrylate has a viscosity of 170,000-220,000 mPa·s at 25° C., a functionality of 1-3, and a number average molecular weight of 70,000-80,000.

[0007] As a preferred embodiment, the aliphatic polyurethane acrylate has a viscosity of 170,000-220,000 mPa·s at 25° C., a functionality of 2, and a number average molecular weight of 72,000.

[0008] As a preferred embodiment, the epoxy-modified acrylate has a viscosity of 25,000-40,000 mPa·s at 25° C., a functionality of 1-3, and a number average molecular weight of 800-1200.

[0009] As a preferred embodiment, the epoxy-modified acrylate has a viscosity of 25,000-40,000 mPa·s at 25° C., a functionality of 2, and a number average molecular weight of 1,200.

[0010] During the experiment, the applicant found that the combination of aliphatic polyurethane acrylate and epoxy-modified acrylate can optimize the electrolyte resistance and prolong the corrosion resistance time in the electrolyte. The possible reason is speculated to be: the polymer structure of the battery protection film polymer prepared by the combination of a difunctional aliphatic polyurethane acrylate with a number average molecular weight of 72,000 and a difunctional epoxy-modified acrylate with a number average molecular weight of 1,200 has dense performance and can achieve electrolyte corrosion resistance. In this application, high number average molecular weight and low number average molecular weight modified acrylic resins are used in combination. On the basis of ensuring the density of the film polymer, it also has good compatible fluidity, can be sealed on the battery surface, improve the adhesion performance of the battery, and reduce the intrusion of the electrolyte.

[0011] As a preferred embodiment, the active diluent is selected from one or a combination of 2-phenoxyethyl acrylate, tetrahydrofurfuryl acrylate, acryloyl morpholine, isobornyl acrylate, trimethylol cyclohexyl acrylate, hexanediol diacrylate, and propoxylated glycerol triacrylate.

[0012] As a preferred embodiment, the active diluent is a combination of tetrahydrofurfuryl acrylate, acryloylmorpholine and propoxylated glyceryl triacrylate.

[0013] As a preferred embodiment, the weight ratio of tetrahydrofurfuryl acrylate, acryloylmorpholine and propoxylated glyceryl triacrylate is (14-18): (8-12): (5-10).

[0014] As a preferred embodiment, the weight ratio of tetrahydrofurfuryl acrylate, acryloylmorpholine and propoxylated glyceryl triacrylate is (15-17): (9-11): (7-9).

[0015] As a preferred embodiment, the weight ratio of tetrahydrofurfuryl acrylate, acryloylmorpholine and propoxylated glyceryl triacrylate is 16:10:8.

[0016] As a preferred embodiment, the initiator is a photoinitiator, and the photoinitiator is selected from one or a combination of initiator 184, initiator TPO, initiator IHT-PI 910, initiator 1173, and initiator 907.

[0017] As a preferred embodiment, the initiator is a combination of initiator 184 and initiator TPO.

[0018] As a preferred embodiment, the weight ratio of the initiator 184 to the initiator TPO is (1-5): (1-3).

[0019] As a preferred embodiment, the weight ratio of the initiator 184 to the initiator TPO is (2-4): (1.5-2.5).

[0020] As a preferred embodiment, the weight ratio of the initiator 184 to the initiator TPO is 3:2.

[0021] As a preferred embodiment, the adhesion promoter is selected from one or a combination of silane adhesion promoters, phosphate acrylate adhesion promoters, and polyester adhesion promoters.

[0022] As a preferred embodiment, the adhesion promoter is a combination of γ-(methacryloyloxy)propyltrimethoxysilane and phosphate acrylate.

[0023] As a preferred embodiment, the weight ratio of the γ-(methacryloyloxy)propyltrimethoxysilane to the phosphate acrylate is (1-3):(1-2).

[0024] As a preferred embodiment, the weight ratio of the γ-(methacryloyloxy)propyltrimethoxysilane to the phosphate acrylate is 2:1.

[0025] As a preferred embodiment, the phosphate acrylate adhesion promoter is trifunctional phosphate acrylate, and the trifunctional phosphate acrylate has a viscosity of 160-320 mPa·s at 25° C. and a number average molecular weight of 150-200.

[0026] As a preferred embodiment, the trifunctional phosphate acrylate has a viscosity of 160-320 mPa·s at 25° C. and a number average molecular weight of 180.

[0027] As a preferred embodiment, the filler is fumed silica, and the fumed silica is hydrophobic fumed silica with a BET-specific surface area of ​​150-250 m 2 / g.

[0028] As a preferred embodiment, the BET specific surface area of ​​the hydrophobic fumed silica is 200 m 2 / g.

[0029] The applicant further discovered during the experiment that the introduction of methoxysilane into the resin system would increase the flocculation viscosity of the resin system, resulting in stratification and flocculation problems and storage instability. However, the introduction of γ-(methacryloyloxy)propyltrimethoxysilane, phosphate acrylate and fumed silica into the resin system could destroy the flocculation effect of methoxysilane on the resin, thereby improving the storage stability of the system.

[0030] A second aspect of the present invention provides a method for preparing an LED-cured battery protective adhesive, comprising the following steps:

[0031] S1. Stir the initiator and the active diluent at 25°C at a speed of 500-1000 r / min until the initiator is completely dissolved;

[0032] S2 then adds filler and stirs thoroughly at 25°C at a speed of 500-1000r / min;

[0033] S3 then adds aliphatic polyurethane acrylate and epoxy modified acrylate, stirs at 1100-1500r / min for 30-50min at 30-50°C, finally adds adhesion promoter and stirs evenly, and disperses under negative pressure in a planetary mixer until defoaming, to obtain battery protective glue.

[0034] Compared with the prior art, the present invention has the following beneficial effects:

[0035] (1) The LED-cured battery protective glue of the present invention adopts a combination of aliphatic polyurethane acrylate and epoxy-modified acrylate, which can optimize the electrolyte resistance performance and prolong the corrosion resistance time in high-temperature electrolyte.

[0036] (2) The LED-cured battery protective glue of the present invention uses a combination of γ-(methacryloyloxy)propyltrimethoxysilane and phosphate acrylate as an adhesion promoter, and is combined with fumed silica to destroy the flocculation effect of the resin system, thereby improving the storage stability of the system.

[0037] (3) The LED-cured battery protective glue of the present invention replaces the anti-rust oil used in traditional battery laser welding holes and uses 395nm LED light curing, which has the advantages of energy saving, environmental protection and high efficiency; at the same time, it can also achieve the salt spray resistance, electrolyte resistance, and super strong adhesion of traditional anti-rust oil. DETAILED DESCRIPTION

[0038] Example 1

[0039] A LED curing battery protective glue, the raw materials for preparation are calculated by weight as shown in Table 1 below:

[0040] Table 1

[0041]

[0042]

[0043] The aliphatic polyurethane acrylate (SR726-1 from Santong Technology) has a viscosity of 170,000-220,000 mPa·s at 25° C., a functionality of 2, and a number average molecular weight of 72,000.

[0044] The epoxy-modified acrylate (Santong Technology ST5035) has a viscosity of 25,000-40,000 mPa·s at 25° C., a functionality of 2, and a number average molecular weight of 1,200.

[0045] The Allnex G3.5POTA is propoxylated glycerol triacrylate; Dow Corning Z-6030 is γ-(methacryloyloxy)propyltrimethoxysilane; and Santong Technology ST1771 is phosphate acrylate, which is a trifunctional phosphate acrylate with a viscosity of 160-320 mPa·s at 25°C and a number average molecular weight of 180.

[0046] The fumed silica Wacker H18 is a hydrophobic fumed silica with a BET specific surface area of ​​200 m 2 / g.

[0047] A method for preparing an LED-cured battery protective adhesive comprises the following steps:

[0048] S1: Stir the initiator and the active diluent at 25°C and 800 r / min until the initiator is completely dissolved;

[0049] S2 then adds filler and stirs thoroughly at 1000r / min at 25°C;

[0050] S3 then adds aliphatic polyurethane acrylate and epoxy modified acrylate, stirs at 1300 r / min at 40°C for 40 min, finally adds adhesion promoter and stirs evenly, and disperses at negative pressure of -0.09 mPa in a planetary mixer until defoaming, to obtain battery protective glue.

[0051] Performance Testing

[0052] 1. Adhesion performance: The products of the embodiments and comparative examples were made into samples, and the adhesion strength was tested according to ASTM D1002 standard after being subjected to -40°C to 100°C thermal shock and 85°C / 85% RH aging.

[0053] 2. Impact performance: The experiment was carried out at 25±1°C. The UV protective glue in the embodiments and comparative examples was evenly coated on the aluminum plate, and the coating thickness was controlled to be 0.2mm. The aluminum plate coated with the battery protective glue was tested for impact resistance by adjusting the impact height of a 1kg hammer with a heavy hammer: such as 40cm, 60cm, 80cm, and 100cm; three different places were tested on each aluminum plate, and the plate was qualified if the UV protective glue was not broken when impacted at 80cm.

[0054] 3. Drop test: The battery protection glue in the embodiment and the comparative example is evenly applied to the laser welding hole at the bottom of the 18650 cylindrical battery with a thickness of 0.2 mm. The battery is dropped from a height of 1.2 m for 20 times. The battery is qualified if there is no debonding or falling off.

[0055] 4. Electrolyte immersion resistance test: The experiment was carried out at 50±1°C. The battery protection glue in the embodiment and the comparative example was evenly coated on the laser welding hole at the bottom of the 18650 cylindrical battery with a thickness of 0.2mm. It was immersed in an electrolyte with a pH of 3 for 72h (3 days) and was qualified if it did not fall off.

[0056] The test results are shown in Table 2.

[0057] Table 2

[0058]

[0059]

[0060] In Example 5 of the present application, Santong SR726-1 polyurethane acrylate and epoxy modified acrylate ST5035 are used to solve the problem of electrolyte immersion resistance. They can be immersed in 50°C electrolyte for 72 hours without falling off, and γ-(methacryloyloxy)propyl trimethoxysilane and phosphate acrylate are introduced as adhesion promoters to solve the storage stability problem of battery protective glue. In the drop test, the battery was dropped from a height of 1.5m at the bottom for 20 times without debonding or falling off, and the result was qualified, with good drop resistance.

Claims

1. An LED-cured battery protective adhesive, characterized in that: The raw materials for preparation include, by weight: 40-65 parts of aliphatic polyurethane acrylate, 10-30 parts of epoxy modified acrylate, 20-55 parts of active diluent, 3-8 parts of initiator, 1-5 parts of adhesion promoter and 1-5 parts of filler.

2. The LED-cured battery protective adhesive according to claim 1, characterized in that: The aliphatic polyurethane acrylate has a viscosity of 170,000-220,000 mPa·s at 25° C., a functionality of 1-3, and a number average molecular weight of 70,000-80,000.

3. The LED-cured battery protective adhesive according to claim 1, characterized in that: The epoxy-modified acrylate has a viscosity of 25000-40000 mPa·s at 25° C., a functionality of 1-3, and a number average molecular weight of 800-1200.

4. The LED-cured battery protective adhesive according to claim 1, characterized in that: The active diluent is selected from one or a combination of 2-phenoxyethyl acrylate, tetrahydrofurfuryl acrylate, acryloyl morpholine, isobornyl acrylate, trihydroxymethyl cyclohexyl acrylate, hexanediol diacrylate, and propoxylated glycerol triacrylate.

5. The LED-cured battery protective adhesive according to claim 4, characterized in that: The active diluent is a combination of tetrahydrofurfuryl acrylate, acryloyl morpholine and propoxylated glyceryl triacrylate.

6. The LED-cured battery protective adhesive according to claim 1, characterized in that: The initiator is a photoinitiator, and the photoinitiator is selected from one of initiator 184, initiator TPO, initiator IHT-PI 910, initiator 1173, initiator 907, or a combination of several of them.

7. The LED-cured battery protective adhesive according to claim 1, characterized in that: The adhesion promoter is selected from one or a combination of silane adhesion promoters, phosphate acrylate adhesion promoters, and polyester adhesion promoters.

8. The LED-cured battery protective adhesive according to claim 7, characterized in that: The phosphate acrylate adhesion promoter is trifunctional phosphate acrylate, and the viscosity of the trifunctional phosphate acrylate at 25° C. is 160-320 mPa·s, and the number average molecular weight is 150-200.

9. The LED-cured battery protective adhesive according to claim 1, characterized in that: The filler is fumed silica, which is hydrophobic fumed silica with a BET specific surface area of ​​150-250 m 2 / g.

10. A method for preparing the LED-cured battery protective adhesive according to any one of claims 1 to 9, characterized in that: The following steps are involved: S1. Stir the initiator and the active diluent at 25°C at a speed of 500-1000 r / min until the initiator is completely dissolved; S2 then adds filler and stirs thoroughly at 25°C at a speed of 500-1000r / min; S3 then adds aliphatic polyurethane acrylate and epoxy modified acrylate, stirs at 1100-1500r / min for 30-50min at 30-50°C, finally adds adhesion promoter and stirs evenly, and disperses under negative pressure in a planetary mixer until defoaming, to obtain battery protective glue.

Citation Information

Patent Citations

  • Glue for battery protective film adhesive tape and preparation method thereof

    CN114702922A

  • Electrolyte-resistant adhesive tape used in lithium battery cell

    CN217438082U