Organic-inorganic composite modified wheat protein adhesive and preparation method thereof

By constructing a hyperbranched epoxy open-ring crosslinking structure and calcium carbonate, combined with the reaction of tannin hyperbranched polymer with wheat protein, the problems of poor water resistance and high viscosity of wheat protein adhesives are solved, and high strength and low cost are achieved Environmentally friendly adhesives meet the performance requirements of artificial board production.

CN118909590APending Publication Date: 2024-11-08INST OF CHEM IND OF FOREST PROD CHINESE ACAD OF FORESTRY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411135970.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing wheat protein adhesives have problems such as poor water resistance, high viscosity and poor processability in the production of artificial boards, which are difficult to meet the strength and performance requirements of industrial applications. The modification method is complex and there may be a risk of formaldehyde release.

Method used

By constructing hyperbranched epoxy ring-open crosslinking synergistic calcium carbonate minerals, combining tannin hyperbranched polymer reacts with wheat proteins, forming an organic-inorganic composite modified wheat protein adhesive, improving its bonding properties and water resistance, and Reduce costs by condensing green and environmentally friendly raw materials such as tannins and citric acid.

Benefits of technology

It significantly improves the bonding and water resistance of wheat protein adhesives, forms a dense network structure, enhances the bonding strength and mildew resistance, meets the needs of environmentally friendly adhesives produced in industrial production, and has a simplified process and low cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_2
    Figure FT_2
Patent Text Reader

Abstract

The invention discloses an organic-inorganic composite modified wheat protein adhesive and a preparation method thereof, the adhesive is prepared from 20-22 parts of vital gluten, 2-2.2 parts of tannin hyperbranched polymer, 1 part of cross-linking agent, 2.2-2.5 parts of calcium carbonate, 5-6 parts of condensed tannin and 65-72 parts of water, and the invention also provides the preparation method of the organic-inorganic composite modified wheat protein adhesive. The hyperbranched tannin polymer, the cross-linking agent and the wheat protein react, the wheat protein is modified, a multiple cross-linking enhancing system is constructed, the bonding performance of the adhesive is effectively improved, the water resistance and environmental protection requirements of the adhesive for the plywood can be met, the practical performance of the wheat protein adhesive is guaranteed, and the application prospect is wide. Meanwhile, the raw materials of the adhesive are biomass, so that the adhesive is low in cost and easy to implement, and is a formaldehyde-free and high-performance wood adhesive.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of biomass adhesives, and specifically relates to an organic-inorganic composite modified wheat protein adhesive and a preparation method thereof. Background Art

[0002] my country is a major producer of wood-based panels, with its output reaching 337 million cubic meters in 2021. In this industry, the consumption of wood adhesives is very large. At present, my country's annual consumption of adhesives for wood-based panels reaches 19 million tons, which is a key core raw material in the production of wood-based panels. The adhesives currently used are mainly petroleum-based urea-formaldehyde resins, phenol-formaldehyde resins and melamine-formaldehyde resins, etc., which mainly have problems such as single product variety and performance, over-reliance on petrochemical raw materials and formaldehyde release. They are also the main source of long-term formaldehyde pollution in plywood. With the continuous improvement of the awareness of the country, industry and consumers on the hazards of formaldehyde, and the further restriction of formaldehyde emissions from wood-based panels by new standards, "formaldehyde-free" wood adhesives have received more and more attention in the field of forest chemical processing and wood-based panel production. It is imperative to develop and utilize bio-based green and environmentally friendly wood adhesives. Plant proteins, cellulose, lignin, tannin, starch, etc. derived from natural products are excellent raw materials for the preparation of formaldehyde-free wood adhesives to replace aldehyde resin adhesives. Among them, wheat protein adhesives have shown great development potential due to their low price, abundant sources, non-toxicity, and convenience in production and use, and have attracted widespread attention in recent years. However, the structural characteristics of wheat protein itself lead to disadvantages such as poor water resistance, high viscosity, and poor processability. The adhesive obtained by the method of single modification of wheat protein often has a bonding strength that is difficult to meet the national requirements for the basic strength performance of artificial boards, and has not been widely used in the field of wood adhesives. In order to improve the performance of wheat protein adhesives to meet the needs of industrial production and application, researchers in the industry have also conducted extensive research. For example, CN202210412354 uses ethanol to denature wheat gluten protein, and then uses glutamine transaminase and epichlorohydrin to modify it to obtain an environmentally friendly wheat gluten protein adhesive. However, this patent requires a large amount of ethanol. CN113684004A utilizes CaO and glutaraldehyde composite modified wheat protein to obtain a kind of improved wheat protein adhesive, improves the adhesive performance of wheat protein adhesive, but glutaraldehyde comes from petrochemical products equally, has the chemical property similar to aldehyde substances, and has certain health risks.As the global attention to environmental protection and sustainable development continues to increase, the development of green, environmentally friendly adhesives has become a research hotspot.Existing research shows that the bonding strength of wheat protein adhesive can be improved to a certain extent by methods such as physics and chemistry, but there are also some problems in the modification method, such as complicated preparation process, poor water resistance, formaldehyde release, etc., in the industrial application production process of plywood, there are still great limitations. Summary of the invention

[0003] The purpose of the present invention is to overcome the deficiencies of the prior art, provide a wheat protein adhesive with excellent water resistance and a preparation method thereof, so as to achieve the purpose of improving the bonding performance of the wheat protein adhesive and meet the market demand for environmentally friendly adhesives.

[0004] In view of this, the present invention provides an organic-inorganic composite modified wheat protein adhesive, studies the active substance with terminal epoxy structure, which can react with the functional groups in wheat protein, and combines the advantages of hyperbranched polymer structure to prepare an organic-inorganic composite modified wheat protein adhesive by constructing hyperbranched epoxy ring-opening cross-linking and synergistic calcium carbonate mineral reinforcement.

[0005] In order to achieve the purpose of the present invention, the present invention adopts the following technical solution:

[0006] The invention discloses an organic-inorganic composite modified wheat protein adhesive, whose raw materials include the following components in parts by weight: 20-22 parts of gluten powder, 2-2.2 parts of tannin hyperbranched polymer, 1 part of crosslinking agent, 2.2-2.5 parts of calcium carbonate, 5-6 parts of condensed tannin and 78-85 parts of water.

[0007] According to the present invention, preferably, the wheat protein content in the gluten powder is greater than 80%;

[0008] According to the present invention, preferably, the condensed tannin is a mixture of bayberry tannin and acacia mangium tannin;

[0009] According to the present invention, preferably, the cross-linking agent is glycerol triglycidyl ether;

[0010] According to the present invention, preferably, the method for preparing calcium carbonate comprises the following steps:

[0011] S1. First, tannic acid was dissolved in water, and then CaCl2 which had been dissolved in aqueous solution was added, and stirred at 800 rpm for 2 h;

[0012] S2. Add a NaCO3 solution in an equal molar amount to the CaCl2 solution into the above tannic acid and CaCl2 solution, stir and react for 24 hours. After the reaction is completed, centrifuge and wash with water to mineralize in situ to generate calcium carbonate.

[0013] According to the present invention, preferably, the tannin hyperbranched polymer is prepared by the following method:

[0014] S1. A certain molar ratio of tannic acid and citric acid is added to a three-necked flask in sequence, and then distilled water is added and heated to reflux at a specific temperature until a viscous brown liquid is obtained, and then a certain amount of distilled water is added thereto. After the citric acid is completely reacted, the reactant is dried in an oven to obtain a tannin polymer (TCA) with a carboxyl terminal;

[0015] S2. After accurately weighing TCA and a certain molar ratio of epichlorohydrin, add them into a three-necked flask equipped with a condenser, a thermometer, and a stirrer, stir and slowly heat up to 120°C. The reaction time is 3 hours. After the reaction is completed, the excess ECH is removed under pressure. When the temperature drops to room temperature, ethyl acetate is added to the three-necked flask, and then sodium hydroxide is added dropwise to the reaction solution. The reaction is carried out at 110-120°C for 5-6 hours. After the reaction is completed, the reaction product is washed three times with water, and anhydrous sodium sulfate is added to dry the product. The solvent in the product is removed by rotary evaporation to obtain a hyperbranched tannin polymer with terminal epoxy groups.

[0016] Further preferably, in the method for preparing the aforementioned hyperbranched tannin polymer, the molar ratio of tannic acid to citric acid is 1:(8-12), preferably 1:10; and the molar ratio of TCA to epichlorohydrin is 1:30.

[0017] The present invention also provides a method for preparing the wheat protein adhesive, comprising the following steps:

[0018] (1) Add gluten and 2.0% SDS to water and pretreat at 25°C for 3 h.

[0019] (2) slowly adding condensed tannin to the pretreatment solution while stirring, adjusting the pH of the mixture to 9-10 with an alkali solution, and then adding the tannin hyperbranched polymer and stirring for 10 minutes;

[0020] (3) adding calcium carbonate and a cross-linking agent, stirring the mixture to make it fully mixed and uniform, and obtaining a modified wheat protein adhesive.

[0021] According to the present invention, preferably, in the aforementioned preparation method, the alkali solution in step (2) is a NaOH solution. Compared with the prior art, the technical solution of the present invention has the following beneficial technical effects:

[0022] (I) The present invention first constructs a tannin hyperbranched polymer, the polymer terminal contains an epoxy group and a carboxyl group, and uses the epoxy group to react with the amino group, carboxyl group and other functional groups on the surface of wheat protein to undergo a ring-opening reaction. At the same time, the calcium carbonate rich in Ca2+ is mineralized in situ. 2+ The catechol structure in the condensed tannin interacts with the protein to form a composite organic-inorganic cross-linked structure, forming a dense network structure, increasing the cross-linking density of the adhesive, and being beneficial to the improvement of the strength of the adhesive. On the basis of having good bonding performance, the water resistance is significantly improved. (ii) The raw material of the present invention contains tannin, which has certain antibacterial properties, can protect the protein matrix, and enhance the mildew resistance of the wheat protein adhesive.

[0023] (III) The condensed tannin, citric acid, gluten powder and the like used in the organic-inorganic modified wheat protein adhesive of the present invention are low-cost, green and environmentally friendly, and are conducive to industrial production. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 This is a SEM image of the cross section of the wheat protein adhesive prepared in Example 1 of the present invention. Experiments have shown that in Example 1, calcium carbonate and hyperbranched tannin polymer are added simultaneously, and the cross section of the adhesive is relatively flat without large holes and gaps.

[0025] Figure 2 The SEM image of the cross section of the wheat protein adhesive prepared in Comparative Example 1 of the present invention shows that the cross section of the adhesive is relatively rough, with a large number of relatively large holes and gaps, which will make it easy for moisture to invade the adhesive. DETAILED DESCRIPTION

[0026] In order to better explain the technical solution of the present invention, the following groups of examples are given for illustration. These examples are only used to describe the present invention, but the content of the present invention is not limited to the following embodiments.

[0027] In the embodiment, the tannin hyperbranched polymer and calcium carbonate are prepared according to the following method:

[0028] The preparation method of the tannin hyperbranched polymer in this embodiment is as follows:

[0029] ① Add 1 mol of tannic acid and 10 mol of citric acid into a three-necked flask in sequence, then add distilled water and heat under reflux at a specific temperature until a viscous brown liquid is obtained, then add a certain amount of distilled water, and after the citric acid is completely reacted, dry the reactants in an oven to obtain a carboxyl-terminated tannin polymer (TCA).

[0030] ② After accurately weighing 0.1 mol of terminal carboxyl TCA and 3 mol of epichlorohydrin, add them to a three-necked flask equipped with a condenser, a thermometer, and a stirrer, stir and slowly heat up to 120°C, the reaction time is 3 hours, after the reaction is completed, the excess ECH is removed under pressure, and when the temperature drops to room temperature, ethyl acetate is added to the three-necked flask, and then sodium hydroxide is added dropwise to the reaction solution, and the reaction is carried out at 110-120°C for 5-6 hours. After the reaction is completed, the reaction product is washed three times with water, and anhydrous sodium sulfate is added to dry the product, and the solvent in the product is removed by rotary evaporation to finally obtain a hyperbranched tannin polymer with terminal epoxy groups.

[0031] The preparation method of inorganic calcium carbonate in the present embodiment is as follows:

[0032] First, tannic acid is dissolved in water, and then CaCl2 that has been dissolved in the aqueous solution in advance is added, and stirred at 800 rpm for 2 hours. NaCO3 solution with an equal molar amount to CaCl2 is added dropwise to the above tannic acid and CaCl2 solution, and stirred for reaction for 24 hours. After the reaction is completed, it is centrifuged and washed with water to form calcium carbonate in situ mineralization. The obtained inorganic material is freeze-dried to obtain a powdered solid.

[0033] Embodiment 1:

[0034] The inorganic-organic modified wheat protein adhesive and the preparation method thereof provided in this embodiment include the following steps:

[0035] (1) Add 20 g of gluten and 2% SDS to 78 g of water and pretreat at 25°C for 3 h;

[0036] (2) slowly adding 5 g of condensed tannin to the pretreatment solution while stirring, adjusting the pH of the mixture to 9-10 with alkali solution, and then adding 2.2 g of tannin hyperbranched polymer and stirring for 10 min;

[0037] (3) Add 2.4 g of calcium carbonate and 1 g of a cross-linking agent, and stir to make the mixture fully mixed to obtain a modified wheat protein adhesive.

[0038] Example 2

[0039] The inorganic-organic modified wheat protein adhesive and the preparation method thereof provided in this embodiment include the following steps:

[0040] (1) Add 22 g of gluten and 2% SDS to 85 g of water and pretreat at 25°C for 3 h;

[0041] (2) slowly adding 6 g of condensed tannin to the pretreatment solution while stirring, adjusting the pH of the mixture to 9-10 with alkaline solution, and then adding 2.0 g of tannin hyperbranched polymer and stirring for 10 min;

[0042] (3) Add 2.2 g of calcium carbonate and 1 g of a cross-linking agent, and stir to mix the mixture thoroughly to obtain a modified wheat protein adhesive.

[0043] Example 3

[0044] The inorganic-organic modified wheat protein adhesive and the preparation method thereof provided in this embodiment include the following steps:

[0045] (1) Add 21 g of gluten and 2% SDS to 83 g of water and pretreat at 25°C for 3 h;

[0046] (2) slowly adding 6 g of condensed tannin to the pretreatment solution while stirring, adjusting the pH of the mixture to 9-10 with alkali solution, and then adding 2.2 g of tannin hyperbranched polymer and stirring for 10 min;

[0047] (3) Add 2.5 g of calcium carbonate and 1 g of a cross-linking agent, and stir the mixture to make it fully mixed and uniform, thereby obtaining a modified wheat protein adhesive.

[0048] Example 4

[0049] The inorganic-organic modified wheat protein adhesive and the preparation method thereof provided in this embodiment include the following steps:

[0050] (1) Add 20 g gluten and 2% SDS to 79 g water and pretreat at 25 °C for 3 h;

[0051] (2) slowly adding 5 g of condensed tannin to the pretreatment solution while stirring, adjusting the pH of the mixture to 9-10 with alkali solution, and then adding 2.1 g of tannin hyperbranched polymer and stirring for 10 min;

[0052] (3) Add 2.3 g of calcium carbonate and 1 g of a cross-linking agent, and stir to make the mixture fully mixed to obtain a modified wheat protein adhesive.

[0053] Comparative Example 1

[0054] (1) Add 20 g gluten and 2% SDS to 79 g water and pretreat at 25 °C for 3 h;

[0055] (2) slowly adding 5 g of condensed tannin to the pretreatment solution while stirring, adjusting the pH of the mixture to 9-10 with alkali solution, and then adding 0 g of tannin hyperbranched polymer and stirring for 10 min;

[0056] (3) Add 0 g of calcium carbonate and 1 g of a cross-linking agent, and stir the mixture to make it fully mixed and uniform to obtain a modified wheat protein adhesive.

[0057] Comparative Example 2

[0058] (1) Add 22 g of gluten and 2% SDS to 85 g of water and pretreat at 25°C for 3 h;

[0059] (2) Slowly adding 6 g of condensed tannin to the pretreatment solution while stirring, adjusting the pH of the mixture to 9-10 with alkali solution, and then adding 2.1 g of tannin hyperbranched polymer and stirring for 10 min;

[0060] (3) Add 0 g of calcium carbonate and 1 g of a cross-linking agent, and stir the mixture to make it fully mixed and uniform to obtain a modified wheat protein adhesive.

[0061] The wheat protein adhesive Examples 1-4 and Comparative Examples 1-2 of the present invention were used to manufacture three-layer plywood, and the process parameters used were as follows:

[0062] Eucalyptus veneer is used, the veneer specifications are 400×400×1.5mm, and the glue amount is 300g / m 2 , the coated veneer is assembled vertically according to the texture direction; the cold pressing pressure is 1.0MPa, the time is 1h; the hot pressing time is 6min, the pressure is 1.0MPa, the temperature is 120℃, and the pressed plywood is placed at room temperature for 24h before performance testing; the water-resistant bonding strength is tested in accordance with the national standard GB / T17657-2013, and the wet shear strength is tested after immersion in (63±3)℃ hot water for 3h and cooling at room temperature. The test results are shown in Table 1.

[0063] Table 1 Bonding strength of three-layer plywood prepared with wheat protein adhesive

[0064] project Example 1 Example 2 Example 3 Example 4 Comparative Example 1 Comparative Example 2 Wet shear strength (MPa) 1.14 1.19 1.21 1.15 0.69 0.76 Dry shear strength (MPa) 1.35 1.42 1.38 1.30 1.36 1.34

[0065] By comparing the wet strength results of Examples 1-4 and Comparative Examples 1-2, it was found that the simultaneous addition of tannin hyperbranched polymer and calcium carbonate helps to synergistically improve the wet bonding strength of the wheat protein adhesive. The water resistance of the plywood prepared using the wheat protein adhesive of the present invention is better than that of the comparative example, and the bonding strength is greater than 0.7 MPa, which meets the strength requirements for Class II indoor plywood in the national standard GB / T17657-2013.

Claims

1. An organic-inorganic composite modified wheat protein adhesive, characterized in that: The raw materials include the following components in parts by weight: 20-22 parts of gluten powder, 2-2.2 parts of tannin hyperbranched polymer, 1 part of crosslinking agent, 2.2-2.5 parts of calcium carbonate, 5-6 parts of condensed tannin and 78-85 parts of water.

2. The organic-inorganic composite modified wheat protein adhesive according to claim 1, characterized in that: The wheat protein content in the gluten powder is greater than 80%.

3. The organic-inorganic composite modified wheat protein adhesive according to claim 1, characterized in that: The condensed tannin is a mixture of bayberry tannin and acacia mangium tannin.

4. The organic-inorganic composite modified wheat protein adhesive according to claim 1, characterized in that: The cross-linking agent is glycerol triglycidyl ether.

5. The organic-inorganic composite modified wheat protein adhesive according to claim 1, characterized in that: The calcium carbonate is prepared by the following method: S1. First, tannic acid was dissolved in water, and then CaCl2 which had been dissolved in aqueous solution was added, and stirred at 800 rpm for 2 h; S2. Then, a NaCO3 solution having an equal molar amount to CaCl2 is added dropwise to the above solution of tannic acid and CaCl2, and the mixture is stirred for reaction for 24 hours. After the reaction is completed, the mixture is centrifuged and washed with water to form calcium carbonate by in-situ mineralization.

6. The organic-inorganic composite modified wheat protein adhesive according to claim 1, characterized in that: The tannin hyperbranched polymer is prepared by the following method: S1. A certain molar ratio of tannic acid and citric acid is added to a three-necked flask in sequence, and then distilled water is added and heated to reflux at a specific temperature until a viscous brown liquid is obtained, and then a certain amount of distilled water is added thereto. After the citric acid is completely reacted, the reactant is dried in an oven to obtain a tannin polymer (TCA) with a carboxyl terminal; S2. After accurately weighing TCA and a certain molar ratio of epichlorohydrin (ECH), add them into a three-necked flask equipped with a condenser, a thermometer, and a stirrer, stir and slowly heat up to 120°C. The reaction time is 3 hours. After the reaction is completed, the excess ECH is removed under pressure. When the temperature drops to room temperature, ethyl acetate is added to the three-necked flask, and then sodium hydroxide is added dropwise to the reaction solution. The reaction is carried out at 110-120°C for 5-6 hours. After the reaction is completed, the reaction product is washed three times with water, and anhydrous sodium sulfate is added to dry the product. The solvent in the product is removed by rotary evaporation to obtain a hyperbranched tannin polymer with terminal epoxy groups.

7. The organic-inorganic composite modified wheat protein adhesive according to claim 6, characterized in that: The molar ratio of the tannic acid to the citric acid is 1:(8-12), preferably 1:10; the molar ratio of the TCA to epichlorohydrin is 1:

30.

8. The method for preparing an organic-inorganic composite modified wheat protein adhesive according to claim 1, characterized in that: The steps include: (1) Add gluten and 2.0% SDS to water and pretreat at 25°C for 3 h; (2) slowly adding condensed tannin to the pretreatment solution while stirring, adjusting the pH of the mixture to 9-10 with an alkali solution, and then adding the tannin hyperbranched polymer and stirring for 10 minutes; (3) adding calcium carbonate and a cross-linking agent, stirring the mixture to make it fully mixed and uniform, and obtaining a modified wheat protein adhesive.

9. The method for preparing an organic-inorganic composite modified wheat protein adhesive according to claim 8, characterized in that: The alkali solution in step (2) is NaOH solution.