Full-bio-based multifunctional material as well as preparation method and application thereof
Through the preparation of all-biologically based multifunctional materials, the reaction of vanillin and cinnamaldehyde to form a reaction between eutectic solvent and tannin acid is solved, and the problem of toxic and harmful substances in existing adhesives and coatings is achieved, and high performance and low cost are achieved , green and environmentally friendly adhesives and coating materials, suitable for density boards and coating fields.
Patent Information
- Application Number
- CN202411247405.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-05
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-09-05
AI Technical Summary
Existing adhesives and coatings often contain volatile toxic compounds, such as formaldehyde, benzene, toluene, etc., which lead to environmental pollution and human health risks. The replacement technology is costly and complex, making it difficult to achieve true green environmental protection.
Using a fully bio-based multifunctional material prepared from eutectic solvents and tannin acid, the eutectic solvent consists of vanillin and cinnamaldehyde, and forms a stable hydrogen bond structure through a certain proportion of mixing, as an adhesive and coating material. The use of organic solvents is avoided, and the "one pot and three-step process" preparation is realized, simplifying the process and reducing costs.
This material has high bonding strength to wood at room temperature, has strong adhesion as an adhesive and coating material, and has better performance than traditional resin adhesives and coatings. It has low cost and simple process, achieving green and environmentally friendly industrial applications.
Smart Images

Figure FT_1 
Figure FT_2 
Figure FT_3
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of adhesives and coatings, in particular to a fully bio-based multifunctional material and a preparation method and application thereof. Background Art
[0002] At present, the commonly used adhesives on the market are mainly urea-formaldehyde resin and phenol-formaldehyde resin, but these adhesives contain formaldehyde, a volatile toxic compound, which is harmful to the human body and the environment. When using these adhesives to prepare density boards, people often cannot use them immediately and need to wait for the formaldehyde to evaporate before using them. Therefore, a green, environmentally friendly, non-toxic and low-cost adhesive is needed.
[0003] In order to solve the adhesive problem, the current technologies to replace these adhesives use lignin to replace phenol, and use furfural, glyoxal and other aldehydes with less toxicity and volatility to replace formaldehyde. However, due to the low activity of lignin, lignin basically needs to be modified. This not only increases the process, but also increases the actual cost, and there is no guarantee that no toxic and harmful substances will be produced in the process, making it difficult to achieve true green environmental protection.
[0004] In addition, the common paint coatings on the market basically contain volatile organic solvents such as formaldehyde, benzene, toluene, etc., which cause serious damage to the human body and also cause great pollution to the environment. People need a non-toxic, harmless, green and low-cost coating to replace them.
[0005] In order to solve this coating problem, water-based coatings are used in related technologies to replace solvent-based coatings. Although water-based coatings solve the problem of volatile organic solvents, they still require petrochemical products such as acrylic acid and polyurethane to synthesize, which is expensive and has a complicated production process. Therefore, people need a non-petroleum-based, low-cost coating to replace them. Summary of the invention
[0006] In view of this, the technical problem to be solved by the present invention is to provide a fully bio-based multifunctional material and a preparation method and application thereof. The fully bio-based multifunctional material provided by the present invention not only has raw materials for preparation that can come from natural biomass materials, is green, environmentally friendly, non-toxic and harmless, but also has multiple functional applications. When used as an adhesive material, it has strong bonding strength to wood or wood raw materials and can be used directly as an adhesive; when used as a coating material, it has strong adhesion to different material substrates.
[0007] The present invention provides a fully bio-based multifunctional material, which is obtained from a deep eutectic solvent and tannic acid;
[0008] The deep eutectic solvent includes vanillin and cinnamaldehyde.
[0009] The low eutectic solvent of the present invention comprises vanillin and cinnamaldehyde, wherein the vanillin is a hydrogen bond donor and the cinnamaldehyde is a hydrogen bond acceptor, and the two are mixed in a certain ratio to form a stable hydrogen bond to obtain a clear and transparent low eutectic solvent. The molar ratio of cinnamaldehyde to vanillin of the present invention is 1: (0.8-1.2), preferably 1: 1. Relevant preliminary experiments show that more or less hydrogen bond donors cannot form a stable hydrogen bond structure.
[0010] The tannic acid, vanillin and cinnamaldehyde of the present invention are all derived from biomass raw materials, which are low in cost, simple and easy to obtain, and avoid the introduction of substances such as phenol and formaldehyde, making the product more environmentally friendly. In certain embodiments of the present invention, the source of the tannic acid includes: pea pods, cork oak or Sicilian sumac leaves, the source of the vanillin compound includes: vanilla beans or beets, and the source of the cinnamaldehyde compound includes: cinnamon bark.
[0011] The present invention also provides a method for preparing the all-bio-based multifunctional material according to any of the above technical solutions, comprising the following steps: reacting a low eutectic solvent and tannic acid to obtain the all-bio-based multifunctional material. The low eutectic solvent and tannic acid in the present invention are the same as those described above and will not be described in detail.
[0012] The low eutectic solvent of the present invention is obtained by mixing vanillin and cinnamaldehyde. Specifically, the low eutectic solvent is obtained by mixing vanillin and cinnamaldehyde in a molar ratio of 1: (0.8~1.2). Preferably, the low eutectic solvent is obtained by mixing vanillin and cinnamaldehyde in a molar ratio of 1:1. The mixing temperature of the present invention is 80°C~100°C, and the mixing time is 20 min~40 min.
[0013] The present invention first reacts a low eutectic solvent and tannic acid. Specifically, the low eutectic solvent and tannic acid are dispersed and then reacted. In certain embodiments of the present invention, tannic acid is evenly dispersed in the low eutectic solvent and then reacted. The dispersion temperature of the present invention is 80°C to 100°C, preferably 90°C, and the dispersion time is 2h to 4h. The present invention mixes vanillin and cinnamaldehyde to prepare a low eutectic solvent, and tannic acid can be dispersed so that tannic acid is fully in contact with the low eutectic solvent, thereby making its reaction more sufficient. In this way, the use of organic solvents can be eliminated, so that the reaction does not produce any waste, and the "one pot three-step method" for preparing materials is realized, which is simple and efficient to operate, produces less three wastes, and is easy to realize industrialization.
[0014] The present invention reacts a low eutectic solvent with tannic acid, the reaction temperature is 120°C to 140°C, and the reaction time is 12 h to 14 h. The present invention raises the temperature to 120 to 140°C in order to reach a temperature at which tannic acid and the low eutectic solvent undergo a polymerization reaction, and the reaction ends after 12 to 14 hours, and an adhesive material with the best performance can be obtained.
[0015] The present invention reacts a low eutectic solvent and tannic acid, specifically reacting the low eutectic solvent, tannic acid and alkaline catalyst in a mass ratio of 1: (1~1.2): (0~0.05), preferably in a mass ratio of 1: 1.1: (0~0.05). In certain embodiments of the present invention, 10 g of a low eutectic solvent, (10~12) g of tannic acid and (0~0.5) g of an alkaline catalyst are reacted. The alkaline catalyst of the present invention includes at least one of sodium hydroxide, sodium carbonate or sodium bicarbonate. If there is too little tannic acid, it cannot react completely with the low eutectic solvent, resulting in an excess of the low eutectic solvent, reducing the viscosity of the system, and thus preventing the product from gelling. If there is too much tannic acid, the excess tannic acid will be doped in the generated material, resulting in a decrease in various properties of the material. Therefore, when the mass ratio of the low eutectic solvent to tannic acid is close to 1: 1.1, the obtained all-biomass-based multifunctional material has the best performance.
[0016] The present invention also provides the use of any of the above-mentioned all-biobased multifunctional materials as an adhesive or coating material. The all-biobased multifunctional material of the present invention can be used as an adhesive, and it can be used directly as an adhesive, or it can be used together with an additive as an adhesive. It has a high bonding strength to poplar boards when used directly as an adhesive. At room temperature, its bonding strength to poplar is 4.7 (± 0.2) MPa, which far exceeds the national standard GB / T 14732-2017 for the bonding strength of phenolic resin wood adhesives ≥ 0.7 MPa. In addition, in the low eutectic solvent and tannic acid used to prepare the all-biobased multifunctional material of the present invention, vanillin is used as a food additive, and cinnamaldehyde is used as a synthetic flavoring for food. They are non-toxic and harmless, low cost, and are excellent substitutes for formaldehyde. Tannic acid, as a natural organic compound, is low cost and is an excellent substitute for phenol. Therefore, compared with phenolic resin and urea-formaldehyde resin adhesives, the all-biomass-based multifunctional material of the present invention is more environmentally friendly, simple in process, and low in cost.
[0017] The all-biobased multifunctional material of the present invention can also be used as a coating material. It can be directly used as a coating material by ultrasonic dispersion in a solvent, or it can be combined with an additive and used as a coating material by ultrasonic dispersion in a solvent, and then the solvent can be dried. The solvent can be selected from at least one of ethanol, water or acetone, preferably ethanol. The mass ratio of the all-biobased multifunctional material to the solvent is 1: (4~9).
[0018] The present invention also provides a product, which can be a glued product, and the glued product is obtained from wood raw materials and adhesives, and the adhesives include the all-biobased multifunctional materials and optional additives described in any of the above technical solutions. In certain embodiments of the present invention, the glued product is a high-performance density board, which is obtained by mixing the all-biobased multifunctional materials and bamboo powder in a mass ratio of 1: (1~3), and then hot pressing at 110℃~130℃ and a pressure of 20 MPa~40 MPa, and then cooling it naturally. The performance of the high-performance density board far exceeds the high-density fiberboard currently on the market, and its bending strength is 44.12 (±2.25) MPa. The bending strength of the high-density fiberboard sold on the market is only 20 (±2.5) MPa. In comparison, the high-performance density board obtained by the present invention has better performance, is greener, and has lower cost. Preferably, the optimal mass ratio of the all-biobased multifunctional material and bamboo powder is 1:2. Preliminary experiments have shown that if there is too much bamboo powder, its performance will decline, and if there is too little bamboo powder, its performance will not improve much, but the cost will increase.
[0019] The product provided by the present invention may also be a coating product, which includes a substrate and a coating disposed on the substrate, and the coating is formed by a coating material including the all-biobased multifunctional material described in any of the above technical solutions and optional additives. The substrate of the present invention includes an iron sheet, a stainless steel plate, a wooden board or a bamboo board, etc. In certain embodiments of the present invention, the all-biobased multifunctional material and ethanol are mixed and ultrasonically dispersed to obtain an ethanol dispersion of the all-biobased multifunctional material, and the dispersion is sprayed on the substrate, dried at 50°C to 70°C for 0.5 h to 1.5 h, preferably dried at 60°C for 1 h, to form a coating on the substrate. The coating formed by the all-biobased multifunctional material described in the present invention has been tested for adhesion, and according to the ASTM D3359-17 standard, its adhesion can reach Class 5B (optimal level).
[0020] The present invention provides a fully bio-based multifunctional material and a preparation method and application thereof. The fully biomass-based multifunctional material provided by the present invention has a strong bonding strength to a poplar board, and the density board prepared using the material and bamboo powder also has a more excellent performance than the current high-density fiberboard, and is an excellent substitute for density boards and plastic boards. The process of preparing a gluing product using the fully bio-based multifunctional material of the present invention is simple, the raw materials are all from plants, non-toxic and harmless, low cost, no by-products are generated in the production process, and it is green and environmentally friendly. It can be used as a safe, reliable, and stable adhesive in furniture and industry, and can improve the quality of adhesives used in wood. It has good economic and social benefits and broad market prospects. Therefore, the fully bio-based multifunctional material of the present invention has broad application prospects as an adhesive in the field of density boards. In addition, the fully biomass-based multifunctional material provided by the present invention has a strong adhesion to iron sheets, stainless steel sheets, wooden boards, bamboo boards, etc. as a coating, and the coating is simple to prepare, non-toxic and harmless, and easy to spray. It is an excellent substitute for organic coatings such as paints and water-based coatings. Therefore, the material also has broad application prospects in the field of coatings. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 A schematic diagram of the bonding strength of the all-biomass-based multifunctional material prepared in Example 1 of the present invention at room temperature;
[0022] Figure 2 A schematic diagram of a density board prepared in Example 2 of the present invention and its bending strength;
[0023] Figure 3 Schematic diagram of the adhesion test of the all-biomass-based multifunctional material prepared in Example 3 of the present invention to an iron sheet. DETAILED DESCRIPTION
[0024] The present invention discloses all-biobased multifunctional materials and preparation methods and applications thereof. Those skilled in the art can refer to the contents of this article and appropriately improve the process parameters for implementation. It is particularly important to point out that all similar substitutions and modifications are obvious to those skilled in the art and are deemed to be included in the present invention. The methods and applications of the present invention have been described through preferred embodiments, and relevant personnel can obviously modify or appropriately change and combine the methods and applications of this article without departing from the content, spirit and scope of the present invention to implement and apply the technology of the present invention.
[0025] The present invention will be further described below in conjunction with embodiments:
[0026] Example 1
[0027] Preparation of all-biomass-based multifunctional materials: 4.9 g of cinnamaldehyde and 5.65 g of vanillin were mixed in a molar ratio of 1:1 and stirred at 90°C for 20 min to obtain a clear and transparent low eutectic solvent. 10 g of tannic acid was added to the low eutectic solvent, and 0.3 g of sodium bicarbonate as a catalyst was added. After stirring for 2 h, when the tannic acid was completely dispersed in the low eutectic solvent, the temperature was raised to 120°C and stirred for 12 h to obtain all-biomass-based multifunctional materials. The mass ratio of the low eutectic solvent to tannic acid was 1:1.
[0028] The bonding strength of the all-biomass-based multifunctional material to the poplar board was tested, and the specific test process is as follows:
[0029] 1) Sample treatment: Take 0.2 g of the all-biomass-based multifunctional material prepared in Example 1 and apply it while hot on about one quarter (15×20 mm 2 ) on a poplar wood chip sample (20 mm×60 mm×3 mm). A portion of the coated sample was placed in a hot press and the sample was hot pressed at 1.5 MPa and 120°C for 10 min, then slowly cooled to room temperature and continued cold pressing for 10 h.
[0030] 2) Room temperature (25°C) bonding performance test: The cold-pressed samples were placed at room temperature for 10 h, and then the samples were subjected to adhesion performance test using a tensile machine at a speed of 5 mm / min. The bonding strength was recorded as the maximum tensile strength.
[0031] like Figure 1 As shown, Figure 1 This is a schematic diagram of the bonding strength of the all-biomass-based multifunctional material prepared in Example 1 of the present invention at room temperature. Figure 1 It can be seen that the all-biomass-based multifunctional material has a strong bonding strength. At room temperature, its bonding strength to the poplar board can reach 4.7 MPa, which far exceeds the bonding strength required by the national regulations for phenolic resin wood adhesives in GB / T14732-2017 (≥0.7 MPa). This shows that the all-biomass-based multifunctional material provided by the present invention can be used as an adhesive to meet the needs of daily life.
[0032] Example 2
[0033] Preparation of high-performance density board: The all-biomass-based multifunctional material obtained in Example 1 is mixed with bamboo powder in a mass ratio of 1:2, and then hot-pressed at 110°C and 20 MPa for 20 min, and then cooled naturally to obtain a high-strength density board. The bending strength test method is the three-point bending method.
[0034] like Figure 2 As shown, Figure 2This is a schematic diagram of the density board prepared in Example 2 of the present invention and its bending strength. Figure 2 It can be seen that its bending strength is 44.21 (±2.25) MPa, which is much higher than the bending strength of the high-density fiberboard sold on the market, which is 20 (±2.5) MPa, indicating that the high-performance density board provided by the present invention can be used as an excellent substitute for high-density board.
[0035] Example 3
[0036] Preparation of all-biomass multifunctional material ethanol dispersion: The all-biomass-based multifunctional material obtained in Example 1 was mixed with ethanol at a mass ratio of 1:4, and then ultrasonicated to form a uniform dispersion, which was sprayed on an iron sheet by spraying, and the ethanol was dried at 60°C for 1 h. After adhesion testing, according to ASTM D3359-17 standard, its adhesion can reach Class 5B (optimal grade).
[0037] like Figure 3 As shown, Figure 3 Schematic diagram of the adhesion test of the all-biomass-based multifunctional material prepared in Example 3 of the present invention to an iron sheet. Figure 3 The left picture shows the coating after being gridded, the middle picture shows the test after the tape is attached to the grid, and the right picture shows the grid after the tape is torn off according to the standard. Figure 3 As can be seen from the three pictures, there is no obvious sign of peeling of the coating in the grid before and after the test. According to the ASTM D3359-17 standard, its adhesion can reach Class 5B (optimal level).
[0038] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. Fully bio-based multifunctional material, characterized in that: It is obtained from a deep eutectic solvent and tannic acid; The deep eutectic solvent includes vanillin and cinnamaldehyde.
2. The all-biobased multifunctional material according to claim 1, characterized in that: The molar ratio of cinnamaldehyde to vanillin is 1:(0.8-1.2).
3. The all-biobased multifunctional material according to claim 1, characterized in that: The tannic acid, vanillin and cinnamaldehyde are all derived from biomass raw materials.
4. The method for preparing the all-biobased multifunctional material according to any one of claims 1 to 3, characterized in that: The following steps are involved: A low eutectic solvent and tannic acid are reacted to obtain a fully bio-based multifunctional material.
5. The method for preparing a fully bio-based multifunctional material according to claim 4, characterized in that: The specific steps include: The low eutectic solvent, tannic acid and alkaline catalyst are reacted in a mass ratio of 1:(1~1.2):(0~0.05) to obtain a fully bio-based multifunctional material.
6. The preparation method according to claim 4, characterized in that: The reaction temperature is 120° C. to 140° C., and the reaction time is 12 h to 14 h.
7. The preparation method according to claim 4, characterized in that: The low eutectic solvent and tannic acid are dispersed and then reacted. The dispersion temperature is 80° C. to 100° C. and the dispersion time is 2 h to 4 h.
8. The preparation method according to claim 4, characterized in that: The deep eutectic solvent is obtained by mixing the cinnamaldehyde and vanillin; The mixing temperature is 80° C. to 100° C., and the mixing time is 20 min to 40 min.
9. Use of the all-biobased multifunctional material described in any one of claims 1 to 3 as an adhesive or coating material.
10. A product, characterized in that The product is a glued product, which is obtained from wood raw materials and adhesives, wherein the adhesives include the all-biobased multifunctional material described in any one of claims 1 to 3 and optional additives; or, The product is a coating product, which includes a substrate and a coating disposed on the substrate, wherein the coating is formed by a coating material comprising the all-biobased multifunctional material described in any one of claims 1 to 3 and optional additives.
Citation Information
Patent Citations
Full-biomass timber adhesive and preparation method as well as application thereof
CN104962227A
Full-biomass wood-bamboo composite material based on tannin bionic crosslinking and preparation method of full-biomass wood-bamboo composite material
CN114426779A
Biomass-base artifical plate wooden adhesive without formaldehyde indoor and production thereof
CN1778857A
IN1411CH2012A
Cited By
Full-bio-based high-performance flame-retardant adhesive based on epoxidized soybean oil / citric acid / tannic acid / nano-hydroxyapatite and preparation method of full-bio-based high-performance flame-retardant adhesive
CN120865838A